Research status

For WC-Co carbide, the rapidly advancing Powder Bed Fusion (PBF) additive manufacturing (AM) technology has shown unique advantages in producing complex structures of metal parts made of carbide. However, when manufacturing WC-Co carbide with high melting points and high content of hard phases, issues such as difficult-to-eliminate cracks, pores, abnormal grain growth, oxidation decarburization, and brittleness often arise, leading to poor mechanical properties of the produced carbide. In recent years, there have been many reports on the use of Green Additive Manufacturing-Debinding and Sintering (GAM-DS) technology to fabricate WC-Co carbide, which have shown significant advantages in addressing issues such as cracking, abnormal grain growth, oxidation decarburization, and brittleness in PBF carbide. However, the process of preparing green bodies is prone to defects such as pores, interlayer cracks, uneven carbon distribution, and weak local bonding, resulting in problems such as porosity, uneven sintering shrinkage, and uneven microstructure in the sintered bodies. Compared with powder metallurgy, the prepared carbide have relatively low relative densities, and there is a significant gap in mechanical properties.

Brief introduction of research results

Recently, the State Key Laboratory of Powder Metallurgy at Central South University has employed Material Extrusion Additive Manufacturing (MEX) – Debinding and Sintering (DS) technology to successfully produce high-strength and tough WC-9Co cemented carbide with no pores, no cracks, and uniform shrinkage in all directions. Its relative density is approximately 99.7%, and its Vickers hardness, transverse fracture strength, and fracture toughness reach 1525±3HV30, 3492±45MPa, and 20.4±0.5 MPa·m1/2 respectively. The comprehensive mechanical properties are comparable to those of high-performance WC-Co carbide prepared by powder metallurgy processes. The relevant work, titled “Material extrusion additive manufacturing of WC-9Co cemented carbide,” was published in the top international journal “Additive Manufacturing.”

 

research chart

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 2

FIG. 1 Microstructure of MEX WC-9Co cemented carbide green

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 3

FIG. 2 Schematic diagram of stack pore formation of cemented carbide printing green billet: a. MEX stack pore formation; b. Increasing the overlap rate of microfilaments is conducive to reducing the stack porosity of green billet;

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 4

FIG. 3 Microstructure of MEX-DSWC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 5

Figure 4 Micro-CT analysis results of internal defects in MEX-DS WC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 6

Figure 5 Microstructure of WC-9Co cemented carbide: (a) MEX-DS; (b) Press forming – degreasing sintering

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 7

Figure 6 MEX-DS WC-Co carbide Co pool and Co rich zone

WC-Co carbide

Figure 7 Transverse fracture strength and fracture toughness of WC-(8-12)Co cemented carbide prepared by different processes

 

Tóm l??c

Conclusion of the Paper

(1) By calculating the plasticity index of the printed feedstock with a powder loading of 54 Vol.%, the mechanism of green body printing defects was analyzed, and the green body MEX parameters were optimized. Using optimized parameters such as a printing temperature of 150°C, filament overlap rate of 30%, and printing layer thickness of 0.1mm, defect-free green bodies of WC-9Co cemented carbide with a relative density of 98.5% were prepared.

(2) Both excessively high or low temperatures during the debinding process using n-heptane can lead to debinding cracks. Rapid solvent evaporation during the drying process of debound bodies can also result in microcracks. By employing a two-step solvent debinding process, namely, n-heptane debinding at 30°C for 12 hours followed by kerosene debinding at 30°C for 1 hour, the solvent evaporation rate was reduced, resulting in high-quality debound bodies with no noticeable debinding defects and uniform distribution of binder.

(3) Defects in MEX green bodies can lead to the formation of Co-rich regions or pools, abnormal WC grains, residual pores, etc., in WC-Co carbide. These defects can be improved or eliminated during the sintering process through liquid phase flow and rearrangement of WC particles. By optimizing the MEX green body printing and solvent debinding processes to eliminate printing and debinding defects, it is possible to eliminate defects such as sintering pores, cracks, Co pools, abnormal grain growth, etc., in WC-Co carbide, resulting in near-full-density WC-9Co carbide.

(4) By employing MEX green bodies, a two-step solvent debinding process, and a continuous thermal debinding-vacuum pressure sintering process, WC-9Co carbide with uniform microstructure, smaller grain size, and relatively uniform distribution were prepared. The Vickers hardness, transverse fracture strength, and fracture toughness were measured to be 1525±3HV30, 3492±45MPa, and 20.4±0.5MPa·m1/2, respectively. The comprehensive mechanical properties were superior to those reported by recent additive manufacturing technologies and comparable to those of WC-Co carbide prepared by traditional powder metallurgy processes.

Main Innovations of the paper of WC-Co carbide additive manufacturing

The use of WC-Co carbide MEX-DS technology to prepare near-full-density WC-9Co carbide, with a transverse fracture strength reaching 3492MPa and a fracture toughness exceeding 20MPa·m1/2, has significantly improved the transverse fracture strength of WC-Co carbide prepared by current AM methods (ranging from 1500-2000 MPa to 3000-4000MPa with HIP treatment) and increased fracture toughness to above 20MPa·m1/2. The comprehensive mechanical properties are significantly better than those reported by similar studies and comparable to similar products prepared by powder metallurgy. The research results are of great significance for addressing the challenging issues of porosity, cracks, and harmful phases encountered in current carbide additive manufacturing and for the development of carbide additive manufacturing technology.

Tr? l?i

Email c?a b?n s? kh?ng ???c hi?n th? c?ng khai. Các tr??ng b?t bu?c ???c ?ánh d?u *

制服丝袜国产在线第一页| 国产伦精品一区二区三区视频抖音| 大黑屌爆操日本女人| 日韩精品高清在线| 亚洲成国产人片在线观看| 日韩美女黄大片在线观看| 美女逼男逼小穴小骚下载| 人妻波多野结衣爽到喷水| 美女穿黑丝被大鸡巴猛操| 干女人逼逼的大几把| 亚洲天堂av一区二区在线观看| 性一交一乱一乱一区二区| 三级片手机在线视频| 国产精品无码av在线一区| 男人摸女人下面视频| 亚洲国产无线码在线| ai换脸久久一区二区亚洲av| 69亚洲一级黄片| 99热这里只有精品亚洲| 大鸡巴日大鸡巴在线观看| 日韩中文字幕一区二区高清| 国产精品视频一区二区三区分享| 最新免费高清无码片| 成人精品视频区一区二区三| 可以免费看黄的香蕉视频| 中文字幕在线观视频| 一区二区三区四区五六区| 胸大裸体美女视频| 91精品国产剧情欧美一区二区| 亚洲国产嫩草18久久久| 欧美亚洲另类天天综合网| 几巴怪物操逼视频| 公交车上被后入搞逼漫画| 日韩人妻精品一区二区三区99| 日韩视频在线网页| 好爽轻点太大了太深了视频| 黑人插中国女人逼| 中文字幕一高清免费视频| 亚洲精品伦理熟女国产| 女人被大鸡吧操逼| 青娱乐欧美性爱视频|