欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

We used metallographic microanalysis and hardness testing methods to study the cause of the failure of cold-punching mould, and proposed an effective measure to improve the life of the mold. Research shows that by optimizing the heat treatment process and processing technology, the material selection is more reasonable and the service life of the mold can be greatly increased.The life of the cold-punching mould is the key factor that can cause the industrial production efficiency failing to improve. The factors that generally lead to die failure include early failures such as chippingand breaking, or serious deformation of the die and no further use. How to improve the die The service life has become a hot topic that the mold industry is highly concerned about.1 Types and Causes of Failure of Cold DiesAccording to the cause of the failure of the mold, the common failure modes can be divided into four failure modes: fracture failure, wear failure, deformation failure, and fatigue failure.Failure formReason for failureFailure failureMold material toughness and strength is not enoughWear failureExcessive wear due to relative motion between the mold and the material being groundDeformation failureMaterial heat treatment deformation, stress concentration, excessive load on the mold, plastic deformation of the materialFatigue failureCracks are continuously generated and expanded under alternating stressCold punching die usually work under difficult and complicated conditions, so die failure is often accompanied by multiple failure modes. Figure 1 starts to crack after stamping 800 pieces.It is made of Cr12MoV wear-resistant high-chromium alloy steel, the design hardness of 55 ~ 58HRC. The quenching process of the mold is (870℃x1.5h + 1050℃x2h) In a vacuum furnace, drawing fire 200℃x 3h. The measured hardness of the mold is shown in Table 2.Fig. 1 Mold partsTable 2 Mold Parts Hardness Test (HRC)Analysis: As can be seen from Table 2, there is a non-uniform distribution of the hardness of the mold parts, which is caused by the uneven heating of the mold during the heat treatment due to the large size of the mold parts. As shown in the metallographic organization chart of Figure 2, the material segregation of the mold parts is very serious due to the insufficient forging during the forging process. There was no macroscopic plastic deformation at the fracture surface and it was granular, and it was judged to be brittle fracture. Figure 2 Metallic microstructureMeasure: Metallographic examination of the metallurgical dimensions is less than 3 levels after full forging. Roughing high-temperature quenching and tempering treatments are added between finishing and finishing. 2 Measures to Improve the Life of Cold Dies 2.1 Reasonable Material SelectionWhen carbon alloy steel is used for brittle fracture due to insufficient plasticity, better tough materials such as microhardened steel 6CrMnNiMoVSi(GD), 9Mn2V steel, low alloy CrWMn steel, 7CrSiMnMoV(CH) steel should be selected. When wear failure is the main failure mode, alloy steels with high carbon content and chromium content (such as Cr12, Cr12MoV), high-carbon medium-chromium alloy steel (Cr8MoWV3Si), 9Cr6W3Mo2V2 (GM) steel, 7Cr7Mo2V2Si (LD) steel, etc. should be used.2.2 Heat Treatment Process ImprovementFirst of all, we must improve the pre-heat treatment process to refine the solid solution of carbides, improve the morphology and distribution of carbides, and increase the plasticity of workpieces. The second is to determine a reasonable quenching conditions, shorten the high-temperature residence time, rotate into the coolant and rotate it to seek even cooling, in order to avoid the failure of the mold.2.3 Reasonable forgingHigh-chromium alloy steels often have severe segregation of carbides and are forged using the cross-draft method. The carbide level after forging is not greater than grade 3. Strictly control the forging temperature and prevent the generation of forging cracks. After the forging, it is often used to anneal the residual heat balls and prepare for the final heat treatment.2.4 Wire cuttingThe size of the wire cutting processing power directly determines the white bright layer thickness and micro-cracks size of the quenched martensite formed on the surface of the workpiece. In the final step of in-line cutting, a small amount of energy is often used for finishing, which can greatly reduce the thickness of the bright white layer and the depth of cracks. After the wire cutting is completed, the mold should be supplemented and tempered to eliminate the additional stress of the wire cutting.3 ConclusionThe working conditions of cold working molds are relatively complex and bad. In the course of use, molds are often intertwined with various kinds of damage. Through the optimization of the heat treatment process and processing technology, the material selection is more reasonable and the service life of the mold can be effectively prolonged.
Ngu?n: Meeyou cacbua

Tr? l?i

Email c?a b?n s? kh?ng ???c hi?n th? c?ng khai. Các tr??ng b?t bu?c ???c ?ánh d?u *

熟妇女人妻丰满中文字幕| 啊好爽好多水深插射视频| 欧美日本大白屁股大黑逼操逼视频| 亚洲综合网伊人中文| 午夜十八禁福利亚洲一区二区| 人妻夜夜添夜夜无码AV| 日本黑鸡吧黄色录像| 天天干天天操天天插| 黄色视频力肏女人| 国产免费无码一区二区视频无码| 日韩激情精品久久久一区二区| 插BB流水水视频| 99久久精品国产一区二区成人了| 性色av少妇一区二区三区多人| 老熟妇高潮一区二区高清视频| 日韩午夜经典福利| 国产 推油 性爱| 欧美一级淫片免费播放口| 波多野结衣高潮尿喷| 日本公共厕所mmm撒尿| 99国产精品一区二区| 中文字幕在线观一区二区| 亚洲精品成a人在线观看| 男人吃奶大鸡巴操逼视频| 亚洲欧美国产原创一区二区三区| 久久99热人妻偷产精品| 天天爽夜夜爽夜夜爽一区| 亚洲人成在线不卡网| 国产熟女视频一区二区三区| 任你橹在线久久精品9| 夫妻性生活视频在线直播| 国产欧美亚洲一区二区三| 九九在线视频热线视频精选| 女生的鸡鸡色色软件| 涩涩屋操美女视频| 99久久久国产精品k影| 欧美激情在线播放第一页| 精品麻豆亚洲欧美| 无码中文字幕免费一区二区三区| 亚洲综合青青草原在线| 狠狠色伊人亚洲综合成人|