Hiper karbür = hiper ala??m + semente karbür

It is well known that there are two important performance indicators for hard metal alloys: hardness and strength. These two factors are often difficult to balance, much like a seesaw. However, the addition of rhenium to high-temperature alloys can significantly enhance the toughness and high-temperature deformation resistance of materials, including iron-based, nickel-based, and cobalt-based high-temperature alloys.

 

Characteristics of hyper?carbide

hyper?carbide?materials, built upon the foundation of general hard metal alloy constituents, incorporate one or several refractory high-temperature metallic components from hyper?alloys, such as rhenium, ruthenium, osmium, molybdenum, vanadium, tantalum, niobium, etc. This modification imparts exceptional characteristics including higher strength, hardness, and temperature resistance compared to conventional hard metal alloys.

One particularly notable effect is observed when trace amounts of rhenium are introduced into hard metal alloys. This addition significantly enhances and improves the physical properties of hard metal alloy materials, particularly in terms of red hardness and alloy stiffness (elastic modulus). Rhenium applies a solid solution strengthening effect to the existing binding phase metals (iron, cobalt, nickel series) in hard metal alloys, particularly in the realm of high-speed cutting and precision machining of challenging-to-process materials like nickel-based high-temperature alloys, heat-resistant stainless steels, titanium alloys, tungsten-molybdenum-tantalum-niobium-zirconium-hafnium class special alloys. The utilization of cutting tools and precision molds made from these newly developed hyper?carbide?materials presents an extraordinary cost-performance advantage, replacing conventional tools in a remarkable manner.

 

The Principle of Rhenium Enhancement in carbide?Performance

People have come to recognize that adding rhenium to the binder of WC-based hard metal alloys can enhance their high-temperature performance.

Figure 1 schematically depicts the W-Co-Re-C phase diagram under conditions of 9wt% Re + 6wt% Co. This diagram, based on literature and experimental results, is compared with a redrawn phase diagram of WC-Co under conditions of 10wt% Co. Considering that the density of Re is significantly higher than that of Co, the WC-Co-Re hard metal alloy with 9wt% Re and 6wt% Co contains almost the same proportion of binder phase in terms of volume as the WC-Co material with 10wt% Co.

From Figure 1, it is evident that the W-Co-Re-C phase diagram differs from the W-Co-C phase diagram. The following are characteristics of the W-Co-Re-C phase diagram:

Fig1 The W-Co-Re-C phase diagram with 9 wt% Re + 6 wt% Co (red line) compared to the W-Co-C phase diagram with 10 wt% Co (black line).
Fig1 The W-Co-Re-C phase diagram with 9 wt% Re + 6 wt% Co (red line) compared to the W-Co-C phase diagram with 10 wt% Co (black line).

Firstly, in the W-Co-Re-C phase diagram, all melting points shift towards higher temperatures. Therefore, compared to traditional WC-Co materials, WC-Co-Re hard metal alloys require sintering at higher temperatures.

Secondly, for WC-Co-Re hard metal alloys, the two-phase region without the η phase and free carbon slightly shifts towards the higher end at higher carbon contents. This shift is relatively minor but still needs to be considered in the preparation of WC-Co-Re hard metal alloys. It’s worth noting that the width of the two-phase regions in the W-Co-Re-C phase diagram is similar to that in the W-Co-C phase diagram.

Lastly, the addition of rhenium to the binder significantly expands the region where the equilibrium of WC + η phase + liquid phase exists at temperatures above approximately 1430°C. This implies that if medium- to low-carbon and low-carbon content WC-Co-Re hard metal alloys are rapidly cooled from the sintering temperature, they might contain the η phase instead of decomposing into thermodynamically stable WC + Co/Re mixtures. Therefore, post-sintering WC-Co-Re hard metal alloys must be cooled at relatively low cooling rates to ensure complete decomposition of the η phase.

Figure 2 illustrates this, showing that batches of WC-Co-Re with medium to low carbon content contain the encapsulated η phase after rapid cooling, while they don’t contain the η phase after slow cooling.

What is Hyper Carbide? 2
Fig2?Under conditions of cooling from the sintering temperature (1520°C) to 1300°C at different cooling rates: (a – cooling rate of 4°C/minute, b – cooling rate of 0.5°C/minute), the microstructure of a medium-grained WC-Co-Re hard metal alloy with 9wt% Re + 6wt% Co and a total carbon content of 5.45 wt%
Hiper Karbür Nedir? 3
Fig3 Sintered at 1520°C, then slowly cooled to 1250°C, the microstructure of medium-grained WC-10%Co hard metal alloy (left) and medium-grained WC-Co-Re (containing 9wt% Re + 6wt% Co) hard metal alloy (right)

Figures 3 and 4 present the typical microstructures of medium-grained WC-Co-Re hard metal alloy, compared to traditional WC-Co materials prepared from the same level of WC powder. From Figure 3, it is evident that the microstructure of WC-Co-Re hard metal alloy is noticeably finer than that of traditional WC-Co hard metal alloy. Thus, rhenium serves as a potent inhibitor of WC grain growth, restraining the coarsening process of WC. According to research findings, rhenium tends to concentrate at the WC/binder grain boundaries. Therefore, it can be inferred that the role of inhibiting WC grain growth in WC-Co-Re materials is analogous to the inhibitory action of traditional grain growth inhibitors at WC-Co interfaces.

Sub-micron WC-Co-Re hard metal alloys are commonly used in high-temperature and high-pressure components, where the role of rhenium in inhibiting grain growth is crucial. This is significant as it eliminates the need to add conventional grain growth inhibitors to sub-micron WC-Co-Re hard metal alloys. Figures 4 and 5 depict the microstructure of sub-micron WC-Co-Re hard metal alloy without grain growth inhibitors, exhibiting fine and uniform particles without exceptionally large WC grains. The sintering temperature for this hard metal alloy is 1520°C, notably higher than the typical sintering temperature for sub-micron WC-Co alloys.

Hiper Karbür Nedir? 4
Figure 4 shows the microstructures of medium-grained WC-Co-Re hard metal alloy with 9 wt% Re + 6 wt% Co (left) and sub-micron WC-Co-Re hard metal alloy with 5.5 wt% Re + 3.7 wt% Co
What is Hyper Carbide? 5
Figure 5 displays the microstructure of sub-micron WC-Co-Re hard metal alloy with 5.5 wt% Re + 3.7 wt% Co.

 

Performance of hyper?carbide?WC-Co-Re

Research has revealed that WC-Co-Re hard metal alloys exhibit significantly improved physical and mechanical properties at high temperatures. The curves in Figure 6 indicate that the hardness of WC-Co-Re material remains more stable as the temperature decreases (20-800°C) compared to traditional WC-Co hard metal alloys. Operating temperatures of 300°C and 500°C are common for HPHT (High Pressure High Temperature) components. In comparison to conventional WC-Co materials, the hardness of WC-Co-Re hard metal alloy reduces by nearly two times at these two temperatures. Increased thermal hardness is crucial for manufacturing tools used for nickel-based high-temperature alloys or other heat-generating materials. These tools require cutting edges with high thermal stability and mechanical robustness.

Hiper Karbür Nedir? 6

Fig. 6. The hardness variation with temperature when comparing sub-micron WC-Co-Re cemented carbide containing 5. 5 wt % Co + 3. 7 wt % Re with traditional sub-micron cemented carbide containing 6 wt % Co

Figure 6 illustrates the variation of hardness with temperature for sub-micron WC-Co-Re hard metal alloy containing 5.5 wt% Co + 3.7 wt% Re, compared to the traditional sub-micron hard metal alloy with 6 wt% Co.

Based on the previously mentioned higher thermal hardness of WC-Co-Re hard metal alloy, it can be inferred that Re-containing hard metal alloys exhibit improved high-temperature creep resistance. In fact, as depicted in Figure 7, the WC-Co-Re hard metal alloy achieves the same compressive stress rate value under a significantly higher load than conventional WC-Co material. This suggests that the Co-Re binder demonstrates significantly enhanced high-temperature creep performance.

Hiper Karbür Nedir? 7

Figure 7 illustrates the relationship between strain rate and compressive stress for WC-Co-Re and WC-Co hard metal alloys at 800°C.

Bir cevap yaz?n

E-posta hesab?n?z yay?mlanmayacak. Gerekli alanlar * ile i?aretlenmi?lerdir

亚洲国产精品伦理在线看| 丰满少妇被强入在线观看| 日本不卡高清视频在线播放| 大鸡巴射在穴穴里的视频| 成年人的一级黄色带| 大鸡巴干小逼视频| 操逼动漫首页登录| 欧美国产三级片久久高清| 国产青青操骚货在线观看| 国产精品白浆一区二区三区| 波多野结衣浴尿解禁在线| 呦交小u女国产精品99| 露脸校花求大鸡巴插| 91成人精品国语自产拍| 精彩欧美一区二区三区| 精品久久久久中文字幕人| 国产裸模大尺度私拍视频| 影音先锋天堂网亚洲无码| 国产精品你懂的在线资源| 可以免费看黄的香蕉视频| 女生的鸡鸡色色软件| 大黑屌后入骚妇屁股| 女人182毛片a级毛片| 亚洲男性天堂一区二区三区| 亚洲精品自拍偷拍第一页| 69国产成人综合久久精| 美女骚逼黄色18禁| 一区二中文字幕在线看国产一区| 色网女人日本逼欧美| 澳门一区二区免费下线观看| 美女大骚逼幸福遍穴| 国产精品亚洲1区2区| 亚洲国产无线码在线| 国产精品一区二区在线观看91| 看一下日本人插逼逼洞视频| av在线国产哟哟| 男人大鸡巴操女人的大逼| 日本最新免费不卡一区二区三区| 亚洲女同一区二区三久久精品| 90岁肥老奶奶毛毛外套| 国产精品毛片无遮挡高清|