Based on the different hard phases, corrosion-resistant cemented carbides can currently be classified into three major categories: WC-based, Cr?C?-based, and TiC-based, with WC-based cemented carbides occupying the largest proportion. Therefore, it is necessary to study the corrosion resistance of this type of alloy. This paper investigates the corrosion resistance of WC-based cemented carbides in acids and alkalis, as well as its relationship with the content and composition of the binder phase, graphite, and η1 phase in the alloy. On this basis, the activated sintering of cemented carbides with low binder phase content is also explored.

Introduction to the Corrosion Resistance of Tungsten Carbides 2

Sample Preparation and Experimental Conditions

Material Selection

To compare the corrosion resistance of WC-based cemented carbides, four groups of test materials were selected:
(1) WC-Co alloy;
(2) WC-Co alloy with a small amount of heterogeneous carbides;
(3) WC-Ni·Mo·Co·Cr alloy;
(4) Low binder phase content alloy.

Corrosion Conditions

Corrosion Media: Hydrochloric acid, sulfuric acid, nitric acid, citric acid (H?Cit), acetic acid (HAC), sodium hydroxide (50%), and potassium hydroxide (50%).
Test Temperatures: 20°C, 40°C, 80°C, and boiling point. Alkali solutions were only tested at the boiling point.
Corrosion Time: 24-72 hours for low temperatures and 6-24 hours for the boiling point.
Corrosion Rate Calculation: The corrosion rate (A) is calculated as the amount of material corroded per unit area per day, expressed in mg/dm2·day (abbreviated as mdd).

Introduction to the Corrosion Resistance of Tungsten Carbides 3

Results and Discussion

Relationship Between Corrosion Rate and Binder Phase Content in WC-Based Cemented Carbides

The corrosion rate of WC-based cemented carbides is related to the content of the binder phase, regardless of the binder’s composition. Alloys with higher binder content exhibit higher corrosion rates. For WC-Co alloys, when the cobalt content exceeds 2%, the corrosion rate increases sharply. In 5% HNO?, the corrosion rate of WC-2% Co alloy still exceeds the acceptable limit. However, the corrosion rate of WC-Ni·Mo·Co·Cr alloy with 2% Ni·Mo·Co·Cr meets the usage requirements under all tested conditions. Even in highly corrosive nitric acid, its corrosion rate is only 196.6 mdd, corresponding to corrosion resistance grade B (less than 250 mdd).

The difference in corrosion rates among alloys with varying cobalt content is not significant at room temperature. However, as the temperature increases, the difference becomes more pronounced. At room temperature, increasing the cobalt content from 2% to 20% results in a corrosion rate change of only 12-30 mdd. At the boiling point, the corrosion rate increases from 20 mdd for low cobalt content to 6×10? mdd for high cobalt content.

Effect of WC Grain Size on Corrosion Rate

Fine-grained alloys have higher interfacial energy and greater internal stress in the binder phase, resulting in lower corrosion resistance. Therefore, fine-grained alloys are not recommended for improving resistance.

Effect of Small Amounts of Heterogeneous Carbides on Corrosion Rate

Comparing WC-Co cemented carbides with small amounts of heterogeneous carbides reveals that their effects on corrosion rates vary:

Cr?C?: A small amount of Cr?C? can improve the alloy’s corrosion resistance. Even though alloy No. 9 has finer WC grains than alloy No. 4, its corrosion resistance is superior due to the addition of Cr?C?.

TaC: The addition of a small amount of TaC has no significant effect on resistance. Comparing alloy No. 4 with alloy No. 7 (which contains 2% TaC), the corrosion rates are similar. Adding 5% TaC also does not improve corrosion resistance.

Mo?C: Adding less than 1% Mo?C can significantly enhance resistance. This is because Mo?C readily dissolves in the γ phase, thereby improving the alloy’s corrosion resistance.

Thus, adding small amounts of Cr?C? or Mo?C is beneficial for improving the corrosion resistance of cemented carbides.

Effect of Graphite and η1 Phase on Alloy Corrosion Rate

The presence of graphite and η1 phase not only significantly affects the physical and mechanical properties of the alloy but also has a notable impact on the corrosion rate. For the tested media, the presence of graphite significantly reduces the alloy’s corrosion resistance. When graphite is present, the solubility of tungsten (or molybdenum) in the binder phase drops below 2-3%, reducing the binder phase’s resistance. Additionally, according to corrosion theory, graphite increases the electrochemical corrosion effect of micro-galvanic cells between phases. Therefore, cemented carbides used as corrosion-resistant materials must avoid the formation of graphite.

In contrast, the η1 phase significantly enhances the alloy’s corrosion resistance. The presence of η1 phase indicates carbon deficiency in the alloy, allowing the binder phase to dissolve a large amount of W (or Mo), typically 10-13%. This composition of the binder phase is more corrosion-resistant. Moreover, the transformation of a certain amount of binder into η1 phase further improves the alloy’s resistance. Thus, under carbon-deficient conditions, the alloy’s corrosion resistance increases sharply compared to normal alloys.

Given these findings, the carbon content should be controlled at the lower limit of the two-phase region or allow the formation of a small amount of dispersed η1 phase, provided that the mechanical properties are not excessively compromised. This results in an ideal microstructure with high corrosion resistance.

Relationship Between Binder Phase Corrosion Resistance and Alloy Corrosion Rate

While the mechanical properties of WC-Ni alloys are generally lower than those of WC-Co alloys, their corrosion resistance is superior, especially under low-carbon conditions. However, alloys with pure nickel as the binder often fail to meet usage requirements, leading to the development of complex nickel-based binders. Ni-Mo alloys exhibit excellent resistance to acid and alkali corrosion, making them suitable as binders for WC-based alloys. This study tested the corrosion resistance of alloys with Ni-Mo-Co-Cr (83:15:1:1) as the binder. The overall trend in corrosion rates for this series is similar to that of WC-Co alloys, but the values are significantly lower. Particularly, low binder content alloys meet the specified usage requirements for all tested media, with corrosion rates below 250 mdd. Additionally, the corrosion rate of WC-Ni·Mo·Co·Cr alloys does not change significantly with increasing temperature.

In summary, improving the corrosion resistance of WC-based cemented carbides depends on enhancing the binder phase’s corrosion resistance, which is particularly effective for low binder content alloys.

Activated Sintering of WC-Based Low Binder Content Alloys

An important approach to improving the resistance of WC-based cemented carbides is to reduce the binder content, provided that the physical and mechanical properties meet usage requirements.

To enhance the performance of sintered products, activated sintering is often employed. The properties of low binder content alloys are closely related to the uniformity of component mixing. Therefore, chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes were adopted. For comparison, conventional processes were also used to prepare alloys with the same composition.

Comparison of Corrosion Resistance Among Different Alloys

Corrosion rates are classified into three grades: A (<25 mdd), B (<250 mdd), and C (<500 mdd). For WC-Co alloys, only low binder content alloys exhibit comprehensive corrosion resistance. In contrast, WC-Ni·Mo·Co·Cr alloys maintain considerable corrosion resistance even with 10% binder content. Notably, WC-2% Ni·Mo·Co·Cr alloys demonstrate excellent resistance under all tested conditions.

WC-Ni·Mo·Co·Cr alloys are widely used in manufacturing ballpoint pen tips. These alloys outperform traditional WC-Co·Ni·Cr alloys in various properties, are easier to produce, and have lower production costs, making them ideal materials for corrosion-resistant ballpoint pen tips.

corrosion resistance

Conclusions

1.The corrosion resistance of WC-based cemented carbides is primarily determined by the resistance of the binder phase. Lower binder content results in better condition. Alloys with Ni·Mo·Co·Cr as the binder exhibit significantly lower corrosion rates than WC-Co alloys, especially those with low binder content.

2.The corrosion rate of WC-based cemented carbides is related to the grain size of the hard phase. Finer grains lead to poorer corrosion resistance.

3.Small amounts of heterogeneous carbides, such as Cr?C? and Mo?C, can improve the resistance of WC-Co alloys, while TaC has little to no effect.

4.Graphite reduces the resistance of WC-based alloys, whereas the η1 phase significantly enhances it. Therefore, the ideal corrosion-resistant alloy should have carbon content controlled at the lower limit of the two-phase region or allow the formation of dispersed η1 phase without excessively compromising mechanical properties.

5.Low binder content alloys with good corrosion resistance can be prepared using chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes, achieving high physical and mechanical properties.

6.The study of the corrosion resistance of WC-based cemented carbides provides a basis for their broader application.

Добавить комментарий

Ваш адрес email не будет опубликован. Обязательные поля помечены *

三上悠亚免费观看在线-青青草原在线视频观看精品| 国产免费高清av在线播放-成年人在线播放中文字幕| 交换朋友的妻子中文字幕-日本美女8x8x8x8| 青木玲高清中文字幕在线看-视频在线免费观看你懂的| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 中文字幕日本在线资源-国产+成+人+亚洲欧洲自线| 欧美字幕一区二区三区-好吊妞欧美一区二区在线观看| 国产日韩电影一区二区三区-美女露双奶头无遮挡物| 国产老熟女激情小视频-成人一区二区人妻不卡视频| 亚洲一区二区三在线观看-国产精品亚洲а∨天堂123| 婷婷亚洲欧美综合丁香亚洲-超刺激国语对白在线视频| 亚洲黑人欧美一区二区三区-亚洲一区二区三区免费视频播放| 少妇一区二区三区粉嫩av-国产精品区久久久久久久| 国内精产熟女自线一二三区-六月丁香婷婷在线观看| 亚洲最新国产无人区123-黄片一区二区在线观看| 欧美精品国产白浆久久正在-国产精彩视频一区二区三区| 日韩亚洲欧美综合在线-成人在线网站在线观看| 国产精品美女在线网址-久草免费福利在线观看视频| 国产福利视频一区二区三区-日韩人妻中文视频精品| 欧美日韩国产在线资源-超碰成人国产一区二区三区| 久久99热这里都是精品啊-国产成人亚洲精品无码aV| av噜噜国产在线观看-欧美视频亚洲视频一区二区三区| 亚洲福利视频免费观看-中文字幕日本不卡一区二区| 日韩精品人妻系列一区-亚洲女同性一区二区三区| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 日韩二级视频在线观看-美女扒开奶罩露出奶子的视频网站| 日韩精品亚洲不卡一区二区-成人网在线视频精品一区二区三区| 成人免费黄色在线网站-日韩精品一区二区三区四区在线| 黄色91av免费在线观看-欧美黄片一级在线观看| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 中文字幕日韩精品不卡一区二区-成人av在线观看一区二区| 国产在线观看高清精品-四季av一区二区三区中文字幕| 久久久精品欧美日韩国产-欧美精品乱码视频在线| 中文字幕日韩不卡久久-五月天中文字幕啊av| 国产精品美女在线网址-久草免费福利在线观看视频| 亚洲av专区在线观看国产-丰满人妻av一区二区三区| 欧美伦乱淫老妇女激情吧-亚洲女邻居精品二区久久| av一区免费在线观看-中文字幕日韩国产精品视频| 中文字幕亚洲综合久久最新-久久精品视频免费久久久| 7m视频7m精品视频网站-亚洲综合香蕉视频在线| 国产精品二区高清在线-91精品91久久久久久|