欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

Milling a thin-walled ring with a composite structure of bilateral axial supporting parts, shown in Figure 1. The material of the part is 30CrMnSiA steel, which complies with the GJB1951-94 standard, and the hardness is 30~35HRC. The surface roughness of the part is Ra=3.2μm, the symmetry of the two supporting parts is 0.05mm, and the perpendicularity of the bottom surface is 0.05mm, indicating high machining requirements. The wall thickness of the ring body is 2mm, which is too thin, leading to insufficient stiffness.

The main body of the part is a weak stiffness structure, which is prone to instability during mechanical machining, especially when machining the outer wall of the ring and clamping the thin-walled ring.

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 2

Machining Analysis

The morphology of the typical weak thin-walled ring with a composite structure of bilateral axial supporting parts after machining with general mechanical machining techniques is shown in Figure 2. The following deficiencies are observed:

(1)Obvious tool marks in the middle of the bilateral axial supporting parts. The upper and lower parts of the bilateral axial supporting parts are formed during two separate machining steps: milling the shape of the thin-walled ring and milling the shape of the bilateral axial supporting parts. Due to the non-coincidence of the process benchmarks between the two steps, obvious tool marks appear in the middle of the bilateral axial supporting parts.

(2)Prominent vibration marks in the middle of the thin-walled ring shape. The wall thickness of the middle part of the ring body is 2mm, which results in significantly insufficient stiffness. During the machining of the thin-walled ring shape, the middle part is prone to instability, leading to the formation of obvious vibration marks. The superposition of these issues collectively results in the machining instability problem becoming a production bottleneck.

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 3

Process Optimization

To address the deficiencies of general mechanical machining techniques, a series of compound machining measures have been adopted, including the conversion control of process benchmarks to “bore-face-contour,” the gradual reduction of workpiece stiffness during machining, the reinforcement of stiffness combined with damping and vibration absorption, and the maximization of clamping area and stiffness. These measures aim to achieve stable machining of the weak thin-walled ring with the composite structure of bilateral axial supporting parts.

Precision Conversion of Process Benchmarks

(1) After rough machining the inner shape and end face, precision turn the inner circle and end face to form the process benchmark “bore-face.”

(2) The specific steps for milling the contour positioning benchmark are as follows.

1)Clamp the fixture in the vise (see Figure 3). The bottom surface of the fixture is aligned with the workpiece end face, and the cylindrical surface of the fixture is aligned with the axial direction of the workpiece inner circle. Use a dial indicator to align the fixture bottom surface with a flatness of ≤0.01mm and then secure it.

2) Clamp the workpiece on the fixture (see Figure 4). The workpiece end face and inner bore are tightly against the fixture’s positioning surface and are clamped with a pressure plate.

 

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 4The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 5

 

3)Symmetrically machine two identical precision milling positioning steps on the workpiece contour (see Figure 5). The step height is 20mm, which converts the process benchmark from “bore-face” to “contour.”

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 6

Steady-state Machining Control

(1) The specific steps for milling the thin-walled ring contour are as follows.

1)Clamp the workpiece with a vice on the precision milling positioning step (see Figure 6).

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 7

2) Embed polytetrafluoroethylene or nylon washers into the internal thread relief groove of the workpiece, and then use an external thread mandrel to screw into the internal thread of the workpiece to enhance the stiffness of the annular body cavity.

3) Machine the round corners of the bilateral supporting parts and the shape of the thin-walled ring (see Figure 7).

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 8

(2) The specific steps for milling the shape of the bilateral axial supporting parts are as follows.

Turn the workpiece around, and use an external thread mandrel (see Figure 8) to screw into the internal thread of the workpiece to enhance the stiffness of the annular body cavity.

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 9

Clamp the workpiece with a clamping block (see Figure 9), and secure it with a flat-nose pliers.

Perform finish machining on the shape of the bilateral axial supporting parts (see Figure 10).

 

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 10

(3) The specific steps for milling the outer step of the bilateral supporting parts?are as follows.

Clamp the fixture with a flat-nose pliers (see Figure 11).

Axially compress the thin-walled ring body of the workpiece with the fixture (see Figure 12).

Press the expanding ring into the inner circle of the workpiece’s thin-walled ring and align the inner circle of the expanding ring with the edge finder.

Machine the structures such as the outer side of the bilateral supporting parts, the step, chamfer, and thread to completion.

The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 11The Milling Method for Thin-Walled Ring and Composite Structures with Weak Stiffness 12

Machining Process

According to the optimized process plan, the specific machining process is as follows.

(1) Milling the profile positioning reference: The milling process for the profile positioning reference is shown in Figure 13.

(2) Milling the shape of the thin-walled ring: The shape of the thin-walled ring after milling is shown in Figure 14.фрезерование

Добавить комментарий

Ваш адрес email не будет опубликован. Обязательные поля помечены *

欧美性做爰片免费视频看| 日韩素人精品亚洲热一区| 美女肏肏逼应用下载| 亚洲国产成人手机版| 国产一二三四五自产| 久久99热人妻偷产精品| 加勒比在线不卡一区二区观看| 日韩欧美人妻综合| av黄色资源在线观看| 日韩美女一区二区三区香蕉视频| 久久噜噜噜久久熟女精品| 久久精精品久久久久噜噜| 一区二区国产精品免费视频| 性一乱一交一免费看视频| 男生的小鸡鸡插进女生的桃子 里| 欧美 日韩 激情 在线| 开心五月播五月亚洲第一| 99热这里有精品在线观看| 男的鸡巴插女的视频| 欧美一区二区三区四公司| 日韩欧美一区二区三区在线视频| 色综合色狠狠天天综合色| 一区二区三区国产l精品欧美| 免费观看的黄视频一级国产| 爱男爽高潮鸡穴视频| 国产精品欧美久久久久久| 粉色av一区二区三区| 婷婷6月天丁香综合在线| 亚洲av熟妇高潮精品啪啪| 男人天堂av在线免费看| 国产成人无码AV一区二区三区| 精品国产自在现线看| 白虎鲍鱼抠逼免费看| 奇米一区二区三区视频在线观看| 精华欧美一区二区久久久| aaa无码偷拍亚洲| ai换脸久久一区二区亚洲av| 中日韩国内精品视频| 国产精品人妇一区二区三区| 开心五月播五月亚洲第一| 另类 专区 综合 中文|