Machining titanium alloy is hard because the thermal conductivity of titanium alloy is very poor. Coupled with the short contact length between the chip and the cutting tool, it is not conducive to the dissipation of cutting heat. As a result, the temperature in the cutting edge region is high, about more than twice that of cutting 45 steel. In addition, tool wear is also severe. On the one hand, the strong chemical affinity between titanium alloy and tool material makes it easy to bond with elements such as Ti, Co, and C in the tool material, aggravating adhesive wear at high temperatures. On the other hand, titanium alloy easily forms a hard and brittle surface layer by reacting with oxygen and nitrogen in the air, exacerbating tool wear.

Table 1: Selection of Tool Geometric Parameters for Turning Titanium Alloys

Инструментальный материал Front Rake Angle ?Back Rake Angle Cutting Edge Inclination Angle Main Clearance Angle Secondary Clearance Angle Chamfer Width (mm) Chamfer Front Angle Cutting Edge Radius (mm)
Carbide lathe 5~10 10~15 0~10 45~75 15 0.05~0.3 0.10~0 0.5~1.5

What are the Challenges in Machining Titanium Alloys? 1

Machining amount

The cutting speed for turning titanium alloys should not be too high, and the cutting depth can be relatively large, while the feed rate should be appropriate. A feed rate that is too large can cause burning of the cutting edge, while a feed rate that is too small results in rapid wear of the cutting edge when processing the hardened layer. When turning titanium alloys, rust-proof emulsion or extreme-pressure emulsion can be used for cooling and lubrication. The recommended cutting parameters for turning titanium alloys are as shown in

Table 2: Selection of Cutting Parameters for Turning Titanium Alloys

Feed (mm) cutting speed(mm)
0.08~0.12 87~69
0.13~0.17 71~59
0.16~0.24 62~51
0.25~0.30 53~47
0.33~0.44 48~41
0.45~0.65 42~34

Note: Conditions for the use of this table: Tool material YG8, workpiece material TC4, tool geometric angles front rake angle = 5°, back rake angle = 10°, main clearance angle = 75°, secondary clearance angle = 15°, cutting edge radius = 0.5mm, turning depth = 1mm, dry turning. If using cutting fluid, the turning speed in the table can be appropriately increased.

What are the Challenges in Machining Titanium Alloys? 2

Machining parameters

Machining Temp.

When turning titanium alloys, the cutting temperature is high, and tool durability is low. Among the cutting parameters, cutting speed has the most significant impact on cutting temperature. Therefore, efforts should be made to ensure that the cutting temperature generated at the selected cutting speed is within the optimal range. The recommended cutting temperature for turning titanium alloys with high-speed steel tools is approximately 480°C to 540°C, while for hard alloy tools, it is around 650°C to 750°C.

Cutting speed Vc

The cutting speed has the most significant impact on tool durability, and it is preferable to operate the tool at the optimal cutting speed with minimal relative wear. When turning titanium alloys of different grades, the cutting speed should be adjusted appropriately due to significant differences in strength. The turning depth also has a certain influence on the cutting speed, and the magnitude of the cutting speed should be determined based on different turning depths.

Feed rate

The feed rate has a relatively small impact on tool durability. While ensuring the machining surface roughness, a larger feed rate can be chosen, typically ranging from f=0.1 to 0.3 mm/r. If the feed rate is too small, the tool may cut within the hardened layer, increasing tool wear. Additionally, extremely thin chips are prone to spontaneous combustion at high cutting temperatures, so a feed rate below f<0.05 mm/r is not allowed.

Cutting depth (ap) has the least impact on tool durability. A larger cutting depth is generally chosen to avoid cutting within the hardened layer, reducing tool wear. It also increases the working length of the cutting edge, promoting heat dissipation. Typically, ap is set at 1 to 5 mm.

Добавить комментарий

Ваш адрес email не будет опубликован. Обязательные поля помечены *

亚洲女同一区二区三久久精品| 天天天天天干夜夜夜夜夜操| 中文字幕人妻一区二区三区人妻| 蜜臀AV无码国产精品尤物| 亚洲国产嫩草18久久久| 男人的天堂久久久久久久| 男人操女人黄片黄色| 免费人成再在线观看| 日韩毛片一区视频免费在线观看| 国产精品无码一二区免费| 操国产骚逼逼逼逼逼逼逼| 国产亚洲精品高清视频免费| 久久久久有精品国产麻豆| 操逼啊 啊 啊黄色视频| 大鸡扒干美女BB直流水| 天堂丝袜人妻中文字幕在线| 亚洲AV无码一区二区三区天堂古| 日韩人妻精品一区二区三区| 亚洲男人的天堂2021| 国精品午夜福利视频导航| 久久久国产精品2020| 成人av大全免费一区二区三区| 国产午夜福利片无码视频| 亚洲中文字幕二区不卡| 91video国产一区| 91成人精品国语自产拍| 在线精品亚洲观看不卡欧| 日本熟人妻中文字幕在线| 色偷偷影音先锋男人av| 国产精品熟女一区二区三区久久夜| 看看美日韩操逼吧| 大鸡巴插美女小逼逼| 国产在线中文字幕一区二区三区| 中文字幕国产精品一区二区三区| 亚洲欧美日韩清纯唯美第一区| 欧美一区二区三区男人的天堂| 精品无码国产一区二区三区A| 激情亚洲人妻精品| 少妇无码一区二区二三区| 欧美日韩国产欧美| 中国毛茸茸的操逼|