For WC-Co w?glik, the rapidly advancing Powder Bed Fusion (PBF) additive manufacturing (AM) technology has shown unique advantages in producing complex structures of metal parts made of carbide. However, when manufacturing WC-Co carbide with high melting points and high content of hard phases, issues such as difficult-to-eliminate cracks, pores, abnormal grain growth, oxidation decarburization, and brittleness often arise, leading to poor mechanical properties of the produced carbide. In recent years, there have been many reports on the use of Green Additive Manufacturing-Debinding and Sintering (GAM-DS) technology to fabricate WC-Co carbide, which have shown significant advantages in addressing issues such as cracking, abnormal grain growth, oxidation decarburization, and brittleness in PBF carbide. However, the process of preparing green bodies is prone to defects such as pores, interlayer cracks, uneven carbon distribution, and weak local bonding, resulting in problems such as porosity, uneven sintering shrinkage, and uneven microstructure in the sintered bodies. Compared with powder metallurgy, the prepared carbide have relatively low relative densities, and there is a significant gap in mechanical properties.

Brief introduction of research results

Recently, the State Key Laboratory of Powder Metallurgy at Central South University has employed Material Extrusion Additive Manufacturing (MEX) – Debinding and Sintering (DS) technology to successfully produce high-strength and tough WC-9Co cemented carbide with no pores, no cracks, and uniform shrinkage in all directions. Its relative density is approximately 99.7%, and its Vickers hardness, transverse fracture strength, and fracture toughness reach 1525±3HV30, 3492±45MPa, and 20.4±0.5 MPa·m1/2 respectively. The comprehensive mechanical properties are comparable to those of high-performance WC-Co carbide prepared by powder metallurgy processes. The relevant work, titled “Material extrusion additive manufacturing of WC-9Co cemented carbide,” was published in the top international journal “Additive Manufacturing.”

 

research chart

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 2

FIG. 1 Microstructure of MEX WC-9Co cemented carbide green

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 3

FIG. 2 Schematic diagram of stack pore formation of cemented carbide printing green billet: a. MEX stack pore formation; b. Increasing the overlap rate of microfilaments is conducive to reducing the stack porosity of green billet;

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 4

FIG. 3 Microstructure of MEX-DSWC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 5

Figure 4 Micro-CT analysis results of internal defects in MEX-DS WC-9Co cemented carbide

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 6

Figure 5 Microstructure of WC-9Co cemented carbide: (a) MEX-DS; (b) Press forming – degreasing sintering

How to achieve a transverse fracture strength of 3492 MPa in high-strength and tough WC-Co carbide additive manufacturing? 7

Figure 6 MEX-DS WC-Co carbide Co pool and Co rich zone

WC-Co carbide

Figure 7 Transverse fracture strength and fracture toughness of WC-(8-12)Co cemented carbide prepared by different processes

 

Podsumowanie

Conclusion of the Paper

(1) By calculating the plasticity index of the printed feedstock with a powder loading of 54 Vol.%, the mechanism of green body printing defects was analyzed, and the green body MEX parameters were optimized. Using optimized parameters such as a printing temperature of 150°C, filament overlap rate of 30%, and printing layer thickness of 0.1mm, defect-free green bodies of WC-9Co cemented carbide with a relative density of 98.5% were prepared.

(2) Both excessively high or low temperatures during the debinding process using n-heptane can lead to debinding cracks. Rapid solvent evaporation during the drying process of debound bodies can also result in microcracks. By employing a two-step solvent debinding process, namely, n-heptane debinding at 30°C for 12 hours followed by kerosene debinding at 30°C for 1 hour, the solvent evaporation rate was reduced, resulting in high-quality debound bodies with no noticeable debinding defects and uniform distribution of binder.

(3) Defects in MEX green bodies can lead to the formation of Co-rich regions or pools, abnormal WC grains, residual pores, etc., in WC-Co carbide. These defects can be improved or eliminated during the sintering process through liquid phase flow and rearrangement of WC particles. By optimizing the MEX green body printing and solvent debinding processes to eliminate printing and debinding defects, it is possible to eliminate defects such as sintering pores, cracks, Co pools, abnormal grain growth, etc., in WC-Co carbide, resulting in near-full-density WC-9Co carbide.

(4) By employing MEX green bodies, a two-step solvent debinding process, and a continuous thermal debinding-vacuum pressure sintering process, WC-9Co carbide with uniform microstructure, smaller grain size, and relatively uniform distribution were prepared. The Vickers hardness, transverse fracture strength, and fracture toughness were measured to be 1525±3HV30, 3492±45MPa, and 20.4±0.5MPa·m1/2, respectively. The comprehensive mechanical properties were superior to those reported by recent additive manufacturing technologies and comparable to those of WC-Co carbide prepared by traditional powder metallurgy processes.

Main Innovations of the paper of WC-Co carbide additive manufacturing

The use of WC-Co carbide MEX-DS technology to prepare near-full-density WC-9Co carbide, with a transverse fracture strength reaching 3492MPa and a fracture toughness exceeding 20MPa·m1/2, has significantly improved the transverse fracture strength of WC-Co carbide prepared by current AM methods (ranging from 1500-2000 MPa to 3000-4000MPa with HIP treatment) and increased fracture toughness to above 20MPa·m1/2. The comprehensive mechanical properties are significantly better than those reported by similar studies and comparable to similar products prepared by powder metallurgy. The research results are of great significance for addressing the challenging issues of porosity, cracks, and harmful phases encountered in current carbide additive manufacturing and for the development of carbide additive manufacturing technology.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

男插女下面高潮视频| 男人扒开女人腿狂躁免费| 国产熟女视频一区二区三区| 97超级免费视频在线观看| 伊人久久亚洲婷婷综合久久| 黄色视频网在线观看| 好想大鸡巴插进阴道视频| 人妻少妇精品视频12p| 日韩美女在线视频一区不卡| 国产精品久久久69粉嫩| 把美女日到高潮喷水视频| 亚洲一区亚洲二区在线观看| 性一交一乱一乱一区二区| 久久久久黑人强伦姧人妻| 熟女大屁股亚洲一区| 国产精品人妇一区二区三区| 精品的极品美女一区二区三区| 亚洲成国产人片在线观看| 枫花恋精品一区二区久久| 女生小穴色色视频| 久久综合色伊人九色91| 丁香社区五月在线视频久| 亚洲国产日韩欧美高清片| 国内精品久久久久精品97| 色熟妇人妻久久中文字幕| 精品少妇一区二区三区中文字幕| 精品麻豆国产免费一区二区三区| 24日本精品视频免费| 麻豆国产欧美一区二区三区r| 男人天堂av在线免费看| 日韩精品诱惑一区?区三区| 在线观看免费视频a v| 男生操女生无马赛克免费| 人妻少妇精品视频12p| 美女的咪咪和骚逼| 欧美日韩在线成人| 无码中文字幕免费一区二区三区| 最新的亚洲欧美中文字幕| 久久69精品久久久久免| 日韩午夜资源在线观看| 女人被躁到高潮嗷嗷叫小|