Inclusions in molten steel during smelting are one of the important reasons for cracks in steel castings. In order to reduce inclusions in molten steel, the smelting operations of deoxidization, desulfuration, impurity removal and degassing should be strengthened in the smelting process, and necessary measures should be taken in the ladle behind the furnace, such as adding rare earth to modify the shape of inclusions, so as to reduce the existence of inclusions and eliminate the cracks of steel castings better.

1. Types and causes of inclusions in steel

Inclusions in steel mainly refer to non-metallic inclusions in steel. It is generally believed that non-metallic inclusions in steel usually exist in the following forms: oxides: F EO, Fe2O3, m no, Al2O3, SiO2, MgO, etc.; sulfides: m ns, FES, etc.; silicates: fesio 4, m nsio 4, FeO · a L2O3 · SiO2, etc.; nitrides: AlN, Si3N4, etc.

The non-metallic inclusions in steel come from two aspects: one is generated along with the smelting process, namely, deoxidizing products of ferroalloy are added during tapping and secondary oxidation products of molten steel and air during pouring, which are called endogenous inclusions, which are generally small particles and evenly distributed in steel; the other is brought in from outside for various reasons, which are called foreign inclusions, This kind of inclusions are mostly irregular in shape, large in size and uneven in distribution, which is the main cause of cracks and is harmful to steel.

Analysis of Crack in Steel Casting 2

The endogenetic inclusions are mainly produced in the following situations: ① in the smelting process, the deoxidized products are not completely eliminated, or the temperature drops during the pouring process, and the deoxidized products generated by the continuous reaction are too late to float and remain in the molten steel, some of them exist in the matrix structure of the steel with small particles, some of them gather into large particles Al2O3), Some of them exist in steel in solid solution state (such as m no and f EO); ② in the process of tapping and pouring, the molten steel is oxidized in contact with air, and oxygen combines with elements in steel to form secondary oxide and remains in the molten steel; during the solidification process of molten steel, FES and FeO with low melting point are separated and crystallized from the molten steel, and finally precipitated at the grain boundary and between dendrites.

Foreign inclusions: this kind of inclusions are mainly brought in by the raw materials, such as sediment, slag and protective slag. The refractory materials of the pouring system are washed and etched by the molten steel, and remain in the molten steel, most of which are large particle inclusions.

The non-metallic inclusions are dissolved in the molten steel or exist in the molten steel alone at high temperature. However, with the decrease of temperature and the change of composition, gas pressure and other conditions, the inclusions originally dissolved in the molten steel will be separated as independent phases and gathered on the grain boundary during the crystallization process, becoming the micro unit for cutting the connection of cast steel matrix and the initial source of cracks, Thus, the potential hidden danger of crack is formed.

2. Relationship between main inclusions and cracks in cast steel and measures to reduce them

In the non-metallic inclusions, the main reason for the cracks of steel castings is sulfide inclusions, which often act together with other factors to increase the crack tendency of steel castings. In cast steel, sulfide inclusions are divided into three types: type I – spherical; type II – point chain like intergranular film; type III – arbitrarily distributed sharp angle. Among them, class II inclusions are the most harmful to steel, class III is the second, and class I is the least. The sulfide inclusions are related to the degree of deoxidization and the amount of residual aluminum in steel. When the amount of aluminum solid solution is low and the amount of oxygen remains little, class I inclusions can be obtained.

Deoxidizer has great influence on the formation of inclusions and the properties of steel. The deoxidizing effect of the composite Deoxidizer is better than that of the single deoxidizer, because the inclusions formed by the composite Deoxidizer are large and easy to float up and remove. If the deoxidation of molten steel is not enough, it is easy to have porosity and crack. However, the amount of aluminum used for final deoxidation is just enough to deoxidize without remaining, the amount of aluminum solid solution is low, and the amount of oxygen remaining is small, which will result in class II inclusions. Generally, excessive aluminum deoxidization will result in class III inclusions. It should be noted that if excessive aluminum is used, more aluminum nitride inclusions will precipitate along the grain boundary, resulting in “rock like” brittle fracture and deterioration of steel properties. Therefore, it is unreasonable to deoxidize with excessive aluminum. The amount of aluminum added and the residual aluminum in steel should not be too low or too high.

Aluminum deoxidization is a widely used method of steel deoxidization. Two deoxidizing processes are usually used in industrial production, one is adding aluminum deoxidizing process, the other is controlling aluminum deoxidizing process. The former is to completely remove the dissolved oxygen in the steel with aluminum, and then remove the Al2O3 inclusion as much as possible through various ways of agitation; the latter is to roughly deoxidize only with silicon manganese, and strictly control the aluminum and calcium content in the steel, so as to control the composition, property and morphology of the oxide inclusion precipitated in the steel [3]. The first deoxidation rate of the former is more than 90, and the deoxidation product is mainly Al 2O 3; the second one is greatly reduced, and the first deoxidation product is mainly SiO2.

Foreign inclusions can be removed according to their sources, while endogenous inclusions need to be controlled by deoxidation and calcium treatment.

In ladle refining, more and smaller argon bubbles are blown into the molten steel to remove the primary deoxidation products.

In order to better remove inclusions and reduce cracks in steel, the following measures are taken for smelting operation.

(1) Prepare raw materials to prevent foreign inclusions.

(2) Adopt reasonable steelmaking process: such as adopt reasonable oxygen blowing and power distribution process, ensure a certain decarburization speed to make inclusions float up, and maintain good furnace condition. (3) Compound Deoxidizer is used instead of single deoxidizer. (4) Adding rare earth in the ladle after the furnace can change the shape of inclusions, reduce inclusions and reduce the cracking of steel castings

Analysis of Crack in Steel Casting 3
高颜值美女视频在线观看| 欧美国产中文高高靖| 高清无码精品一区二区三区| 三级片手机在线视频| 欧美区 日韩区 亚洲区| 女人被躁到高潮嗷嗷叫小| 一区二区三区中文字幕免费在线| 黄网官方在线观看| 黑人大鸡把操逼视频| 中文字幕人妻一区二区三区久久| 女人被躁到高潮嗷嗷叫小| —级v免费大片欧美| 伊人久久丁香色婷婷啪啪| 看小伙草白女人比的黄片| 大鸡巴操屁眼无码| 午夜成人理论片在线观看| 亚洲男人的天堂2021| 找个日韩操逼的看看| 欧美人与动人物A级| 国产在线麻豆精品| 中国毛茸茸的操逼| 老湿机69福免费破解版| 99久久精品国产一区二区成人了| 国产一区二区三区三级88| 插BB流水水视频| 男生狂操女生污视频| 国产操小骚逼视频| 无码人妻精品一区二区三区蜜桃| 欧美性爱撅臀插入啪啪啪| 极品 操 抽插视频| 国产裸模大尺度私拍视频| 日韩久久中文字幕| 操俄罗斯美女bb| 国产一区二区在线观看精品| 欧美日韩精品视频在线第一区| 国产精品熟女一区二区三区久久夜| 熟女菊蕾老妇俱乐部视频| 国产色哟哟精选在线播放| 大鸡巴射精在小穴动漫版| 99国产精品一区二区| 精品麻豆亚洲欧美|