Based on the different hard phases, corrosion-resistant cemented carbides can currently be classified into three major categories: WC-based, Cr?C?-based, and TiC-based, with WC-based cemented carbides occupying the largest proportion. Therefore, it is necessary to study the corrosion resistance of this type of alloy. This paper investigates the corrosion resistance of WC-based cemented carbides in acids and alkalis, as well as its relationship with the content and composition of the binder phase, graphite, and η1 phase in the alloy. On this basis, the activated sintering of cemented carbides with low binder phase content is also explored.

Introduction to the Corrosion Resistance of Tungsten Carbides 2

Sample Preparation and Experimental Conditions

Material Selection

To compare the corrosion resistance of WC-based cemented carbides, four groups of test materials were selected:
(1) WC-Co alloy;
(2) WC-Co alloy with a small amount of heterogeneous carbides;
(3) WC-Ni·Mo·Co·Cr alloy;
(4) Low binder phase content alloy.

Corrosion Conditions

Corrosion Media: Hydrochloric acid, sulfuric acid, nitric acid, citric acid (H?Cit), acetic acid (HAC), sodium hydroxide (50%), and potassium hydroxide (50%).
Test Temperatures: 20°C, 40°C, 80°C, and boiling point. Alkali solutions were only tested at the boiling point.
Corrosion Time: 24-72 hours for low temperatures and 6-24 hours for the boiling point.
Corrosion Rate Calculation: The corrosion rate (A) is calculated as the amount of material corroded per unit area per day, expressed in mg/dm2·day (abbreviated as mdd).

Introduction to the Corrosion Resistance of Tungsten Carbides 3

Results and Discussion

Relationship Between Corrosion Rate and Binder Phase Content in WC-Based Cemented Carbides

The corrosion rate of WC-based cemented carbides is related to the content of the binder phase, regardless of the binder’s composition. Alloys with higher binder content exhibit higher corrosion rates. For WC-Co alloys, when the cobalt content exceeds 2%, the corrosion rate increases sharply. In 5% HNO?, the corrosion rate of WC-2% Co alloy still exceeds the acceptable limit. However, the corrosion rate of WC-Ni·Mo·Co·Cr alloy with 2% Ni·Mo·Co·Cr meets the usage requirements under all tested conditions. Even in highly corrosive nitric acid, its corrosion rate is only 196.6 mdd, corresponding to corrosion resistance grade B (less than 250 mdd).

The difference in corrosion rates among alloys with varying cobalt content is not significant at room temperature. However, as the temperature increases, the difference becomes more pronounced. At room temperature, increasing the cobalt content from 2% to 20% results in a corrosion rate change of only 12-30 mdd. At the boiling point, the corrosion rate increases from 20 mdd for low cobalt content to 6×10? mdd for high cobalt content.

Effect of WC Grain Size on Corrosion Rate

Fine-grained alloys have higher interfacial energy and greater internal stress in the binder phase, resulting in lower corrosion resistance. Therefore, fine-grained alloys are not recommended for improving resistance.

Effect of Small Amounts of Heterogeneous Carbides on Corrosion Rate

Comparing WC-Co cemented carbides with small amounts of heterogeneous carbides reveals that their effects on corrosion rates vary:

Cr?C?: A small amount of Cr?C? can improve the alloy’s corrosion resistance. Even though alloy No. 9 has finer WC grains than alloy No. 4, its corrosion resistance is superior due to the addition of Cr?C?.

TaC: The addition of a small amount of TaC has no significant effect on resistance. Comparing alloy No. 4 with alloy No. 7 (which contains 2% TaC), the corrosion rates are similar. Adding 5% TaC also does not improve corrosion resistance.

Mo?C: Adding less than 1% Mo?C can significantly enhance resistance. This is because Mo?C readily dissolves in the γ phase, thereby improving the alloy’s corrosion resistance.

Thus, adding small amounts of Cr?C? or Mo?C is beneficial for improving the corrosion resistance of cemented carbides.

Effect of Graphite and η1 Phase on Alloy Corrosion Rate

The presence of graphite and η1 phase not only significantly affects the physical and mechanical properties of the alloy but also has a notable impact on the corrosion rate. For the tested media, the presence of graphite significantly reduces the alloy’s corrosion resistance. When graphite is present, the solubility of tungsten (or molybdenum) in the binder phase drops below 2-3%, reducing the binder phase’s resistance. Additionally, according to corrosion theory, graphite increases the electrochemical corrosion effect of micro-galvanic cells between phases. Therefore, cemented carbides used as corrosion-resistant materials must avoid the formation of graphite.

In contrast, the η1 phase significantly enhances the alloy’s corrosion resistance. The presence of η1 phase indicates carbon deficiency in the alloy, allowing the binder phase to dissolve a large amount of W (or Mo), typically 10-13%. This composition of the binder phase is more corrosion-resistant. Moreover, the transformation of a certain amount of binder into η1 phase further improves the alloy’s resistance. Thus, under carbon-deficient conditions, the alloy’s corrosion resistance increases sharply compared to normal alloys.

Given these findings, the carbon content should be controlled at the lower limit of the two-phase region or allow the formation of a small amount of dispersed η1 phase, provided that the mechanical properties are not excessively compromised. This results in an ideal microstructure with high corrosion resistance.

Relationship Between Binder Phase Corrosion Resistance and Alloy Corrosion Rate

While the mechanical properties of WC-Ni alloys are generally lower than those of WC-Co alloys, their corrosion resistance is superior, especially under low-carbon conditions. However, alloys with pure nickel as the binder often fail to meet usage requirements, leading to the development of complex nickel-based binders. Ni-Mo alloys exhibit excellent resistance to acid and alkali corrosion, making them suitable as binders for WC-based alloys. This study tested the corrosion resistance of alloys with Ni-Mo-Co-Cr (83:15:1:1) as the binder. The overall trend in corrosion rates for this series is similar to that of WC-Co alloys, but the values are significantly lower. Particularly, low binder content alloys meet the specified usage requirements for all tested media, with corrosion rates below 250 mdd. Additionally, the corrosion rate of WC-Ni·Mo·Co·Cr alloys does not change significantly with increasing temperature.

In summary, improving the corrosion resistance of WC-based cemented carbides depends on enhancing the binder phase’s corrosion resistance, which is particularly effective for low binder content alloys.

Activated Sintering of WC-Based Low Binder Content Alloys

An important approach to improving the resistance of WC-based cemented carbides is to reduce the binder content, provided that the physical and mechanical properties meet usage requirements.

To enhance the performance of sintered products, activated sintering is often employed. The properties of low binder content alloys are closely related to the uniformity of component mixing. Therefore, chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes were adopted. For comparison, conventional processes were also used to prepare alloys with the same composition.

Comparison of Corrosion Resistance Among Different Alloys

Corrosion rates are classified into three grades: A (<25 mdd), B (<250 mdd), and C (<500 mdd). For WC-Co alloys, only low binder content alloys exhibit comprehensive corrosion resistance. In contrast, WC-Ni·Mo·Co·Cr alloys maintain considerable corrosion resistance even with 10% binder content. Notably, WC-2% Ni·Mo·Co·Cr alloys demonstrate excellent resistance under all tested conditions.

WC-Ni·Mo·Co·Cr alloys are widely used in manufacturing ballpoint pen tips. These alloys outperform traditional WC-Co·Ni·Cr alloys in various properties, are easier to produce, and have lower production costs, making them ideal materials for corrosion-resistant ballpoint pen tips.

corrosion resistance

Conclusions

1.The corrosion resistance of WC-based cemented carbides is primarily determined by the resistance of the binder phase. Lower binder content results in better condition. Alloys with Ni·Mo·Co·Cr as the binder exhibit significantly lower corrosion rates than WC-Co alloys, especially those with low binder content.

2.The corrosion rate of WC-based cemented carbides is related to the grain size of the hard phase. Finer grains lead to poorer corrosion resistance.

3.Small amounts of heterogeneous carbides, such as Cr?C? and Mo?C, can improve the resistance of WC-Co alloys, while TaC has little to no effect.

4.Graphite reduces the resistance of WC-based alloys, whereas the η1 phase significantly enhances it. Therefore, the ideal corrosion-resistant alloy should have carbon content controlled at the lower limit of the two-phase region or allow the formation of dispersed η1 phase without excessively compromising mechanical properties.

5.Low binder content alloys with good corrosion resistance can be prepared using chemical mixing to produce composite powders, intensified ball milling, and activated sintering processes, achieving high physical and mechanical properties.

6.The study of the corrosion resistance of WC-based cemented carbides provides a basis for their broader application.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

7m视频7m精品视频网站-亚洲综合香蕉视频在线| hd在线观看一区二区-免费一区二区三区毛片在线| 天天干天天日天天射天天舔-精品香蕉视频官网在线观看| 精品少妇一区二区18-一区二区三区日韩在线播放| 亚洲欧洲成视频免费观看-国产福利一区二区在线观看| 亚洲国产精品日韩欧美-国产又粗又硬又大爽黄| 欧美精品一区二区不卡-精品国产一区二区三区香蕉网址| 亚洲永久免费在线观看-亚洲欧美导航一区二区导航| 九九热这里只有精品九九-欧美日韩人妻精品一二三| 三上悠亚免费观看在线-青青草原在线视频观看精品| 三级a级一级大片在线观看-日韩av有码免费观看| 日韩毛片在线免费人视频-超碰中文字幕av在线| 在线免费观看黄片喷水-国产精品白丝网站在线观看| 中文字幕日韩精品不卡在线一区-国产tv日韩在线观看视频| 欧美精品啪啪人妻一区二区-嫩草人妻舔舔羞羞一区二区三区| 性色国产成人久久久精品二区三区-偷窥中国美女洗澡视频| 少妇人妻无码久久久久久-综合图片亚洲网友自拍| 欧美三级韩国三级日本三斤-日本不卡一区不卡二区| 国产人妻人伦精品日本-国产98超碰人人做人人爱| 蜜臀av日日欢夜夜爽一区-av在线免费永久播放| 一级特黄大片亚洲高清-国产精品视频伊人久久| 亚洲欧美精品在线一区-99热国产在线手机精品99| 欧美日本亚一级二级三区久久精品-日韩欧美一区二区久久婷婷| 欧美一级一线在线观看-亚洲一区二区亚洲三区| 色噜噜噜噜一区二区三区-欧美最猛黑人做爰视频| 日韩综合精品一区二区-丝袜美腿熟女人妻经典三级| 久久高清超碰av热热久久-国产高清不卡免费视频| 久久特一级av黄色片-91社区视频免费观看| 中文字幕人妻少妇第一页-隔壁的女孩在线看中文字幕| 欧美精品国产白浆久久正在-国产精彩视频一区二区三区| 五月婷婷免费观看视频-男人操女人下面视频在线免费看| 免费午夜福利视频在线观看-亚洲成人日韩欧美伊人一区| 狠狠狠狠爱精品一二三四区-l舌熟女av国产精品| 精品少妇一区二区18-一区二区三区日韩在线播放| 国产在线一区二区三区欧美-久久偷拍精品视频久久| 日韩精品亚洲不卡一区二区-成人网在线视频精品一区二区三区| 久久蜜桃精品一区二区-麻豆视频啊啊啊好舒服| 国产精品熟女视频一区二区-国产日韩精品欧美一区喷水| 日韩av电影一区二区网址-老熟妇仑乱视频一区二| 欧美日韩国产综合四区-爆操极品尤物熟妇14p| 国产成人精品免费视频大全办公室-亚洲欧美日本综合在线|