TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

3 aspekty, które wp?ywaj? na temperatur? spiekania Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

Wniosek

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

Dodaj komentarz

Twój adres email nie zostanie opublikowany. Pola, których wype?nienie jest wymagane, s? oznaczone symbolem *

大鸡巴插入阴道视频| 日韩欧美综合一二三区| 丁香婷婷亚洲六月综合色| 亚洲av 又黄又爽十大| 日本免费无码一区二区到五区| 大鸡巴操逼 公司| 男人的下面进女人的下面在线观看| 裸体美女被操的啊啊直叫| 猛哥操女人B视频| 中日美女毛5片一区二区三区| 伊人网在线免费视频| 精彩欧美一区二区三区| 久久精品男人的天堂av| 国语自产免费精品视频在| 精品久久av免费一区二区三区| 色偷偷影音先锋男人av| 浪潮AV色综合久久天堂| 色网女人日本逼欧美| 大鸡巴狂插嫩逼视频| 色综合色狠狠天天综合色| 999精品免费视频| 99精品一级欧美片免费| 大鸡吧视频在线观看| 精品v欧洲高清欧美| 欧美亚洲综合久久夜夜嗨| 日韩欧美中文字幕国产精品| 黑人大鸡巴双插美女| 女人18片毛片。| 蜜臀AV无码国产精品尤物| 日本一区二区三区高潮喷吹| 日本黑鸡吧黄色录像| 国产高清乱码女大生AV| 被医生添奶头和下面好爽| 久久久久人妻一区精品加勒比| 国产 欧美 日韩 黄片| 亚洲一区二区三区日本在线| 啊啊啊别操了视频| 阴茎大头插少妇蜜穴视频| 国产羞羞的视频在线观看| 亚洲国产国产综合一区首页| 欧美日韩国产这里只有精品|