As with traditional machining methods, EDM machining of cemented carbide will cause carbide cracks initiation as well, but engineers often ignore this fact because WEDM is high-precision machining. We often use WEDM to process cemented carbide products that are small in size, complex in shape and cannot be processed by grinding wheel. However, engineers generally take dimensional accuracy, surface roughness and production efficiency into consideration while ignore the influence of WEDM on the micro-structure area of the carbide surface.

 

Carbide crack initiation mechanism

Different from general machining, the wire cutting wire doesn’t contact the work piece directly, but gradually erodes the metal material by the continuous pulse spark discharge generated between them. In WEDM, the temperature of the machined surface changes rapidly and lead to uneven stress on work piece. This situation is particularly at ease to occur in the processing of hard and brittle materials, such as cemented carbide, cermets, etc. In past empirical research ,When the electrical parameters are not set up properly, crack initiation will appear on the surface of the work piece once the thermal stress exceeds the strength limit.

pic of how wedm working on carbide and produce carbide initiation

According to the thermal stress model, the amount of heat entering the material is proportional to the peak stress. This heat is directly related to the input electric pulse energy under the same other conditions, which is that the greater the input power, the more heat the material absorbs and the greater the stress. Under the condition of neglecting the energy loss, the energy acting on the workpiece during processing can be simplified as below,

3 Significant Factors Making Carbide Crack Initiation of Carbide Product in WEDM 1

In this formula, W is the pulse energy (J); U is the intermittent instantaneous discharge voltage (V); I is intermittent instantaneous discharge current (A); T is the time (s); Tk is the discharge duration (pulse width, s).

In this formula, W is the pulse energy (J).U is the intermittent instantaneous discharge voltage (V).I is intermittent instantaneous discharge current (A).T is the time (s). Tk is the discharge duration (pulse width, s).

It can be seen from the formula that when the discharge duration (pulse width) is determined, increasing the discharge voltage and current will aggravate the crack initiation. When the discharge voltage and current are determined, increasing the discharge duration (pulse width) will result in the same outcome.

 

Experiment plant of micro crack initiation on carbide

A bunch of cemented carbide bushings (see Figure 2) ,made of YG6 cemented carbide (Chinese carbide grade), will be processed for the experiment. ?The bushing’s in height of 30mm, with key slots in width of 1.6mm and depth of 1mm. After being processed, the bushings will be made into metallography sample for SEM inspection to observe the crack initiation and propagation on the machined surface of cemented carbide。

WEDM における超硬製品の超硬クラックの開始をもたらす 3 つの重要な要因 2

In the test, the medium wire cutting equipment CTP350 is used. The cutting fluid is emulsion with a concentration of 8%, and the cutting wire is φ 0.18mm molybdenum wire, one piece is clamped at a time for processing, and the processing parameters of wire cutting are shown in Table 1.

Other main test condition:
edm machine: CTP350
cooling fluid: 8% emulsion
cutting wire:φ0.18 molybdenum wire
processing times limit: 1 piece a time
and WEDM processing set-up parameters are shown in the following table 1.

3 Significant Factors Making Carbide Crack Initiation of Carbide Product in WEDM 3

The test result about WEDM carbide crack initiation involving 4 factors

Electricity pulse width

Metallographic photos of 1 #~4 # products are shown in Fig. 3~Fig. 6. It can be seen from the figure that with the decrease of pulse width, the microcracks on the alloy surface gradually become smaller. When the pulse width is 40ms, the depth of microcrack reaches mmmm; When the pulse width is 12 ms, there is basically no crack initiation.

WEDM における超硬製品の超硬クラックの開始をもたらす 3 つの重要な要因 4

Electricity current value

The metallographic photos of 5 #~8 # products are shown in Fig. 7~Fig. 10. It can be seen that when the processing current is 3.5A, the crack depth is more than 30mm; When the processing current is 2.8A, the crack depth is 30mm; When the processing current is 2.4A, the crack depth is 20mm; While the processing current is 2.0A, the crack depth is 10mm. All in all, the greater the machining current, the greater the crack depth.

3 Significant Factors Making Carbide Crack Initiation of Carbide Product in WEDM 5

Voltage

The metallographic photos of product 9# ~ 12# are shown in Figure 11 ~ 14.?It can be seen that when the current is 2A, the pulse width is 20μm, and the pulse interval is 8 times the pulse width, the processing voltage is 70 ~ 120V, and no alloy microcracks are found in the cutting section. In other words, the influence of voltage on the carbide crack?initiation?is not obvious when the current and pulse width are constant.

WEDM における超硬製品の超硬クラックの開始をもたらす 3 つの重要な要因 6

Cutting times

The metallographic photos of 13 #~15 # products are shown in Figures 15~17. It can be seen that through multiple cutting processes, the surface quality of the product become better and micro-crack’s depth gradually reduced as cutting times grow. The depth of the micro-crack of the product is within 15mm after two times of WEDM processing; The depth of micro-cracks in the product is within 10mm after three times of WEDM processing. Thus, through two times of cutting processing, it can meet the requirement that the micro-crack depth of carbide bushing should be less than 20mm.

WEDM における超硬製品の超硬クラックの開始を引き起こす 3 つの重要な要因 7

The experimental summary of cracks in cemented carbide produced by WEDM

When WEDM is used to process brittle materials such as cemented carbide, the pulse width and processing current have obvious effects on the microcracks on the surface of the alloy, which are shown in the following aspects: the greater the pulse width and current, the deeper the crack. However, the effect of voltage on the surface microcracks of the alloy is not obvious. No microcracks were found when the pulse width was 12 μm.

When the working current is above 2A, the workpiece will have cracks to a certain extent. Therefore, when selecting electrical parameters, avoid selecting the processing current above 2A. The superposition effect of temperature field should be fully used to reduce the size of thermal stress and its impact property, so that the workpiece material can be thrown out in gas phase to avoid overheating of the workpiece surface.

In addition, multiple cutting is a very effective method to reduce and remove surface microcracks.

コメントを殘す

メールアドレスが公開されることはありません。 が付いている欄は必須項目です

久久久18禁一区二区网| 日本六十五十熟女一级黄色| 精品精品国产一区二区性色av| 热精品韩国毛久久久久久| 日本亚欧乱色视频69室| 91成人精品国语自产拍| 国产日女人视频在线观看| 高颜值美女视频在线观看| 国产情侣色综合久久有码| 亚洲AV天堂一区二区香蕉| 大鸡巴干浪穴视频| 最是人间烟火色在线播放| 捆绑调教白浆一区二区三区| 色噜噜噜噜一区二区三区| 插插插插插插插插插插插| av在线国产哟哟| 3色w九九久久男人皇宫宕| 一区二区三区 日韩在线| 男插女逼啪啪啪软件| 国产无圣光一区福利二区| 胸大裸体美女视频| 天堂久久久久久久久久久| 西瓜在线看免费观看视频| 天天舔操操操av| 国产欧美一区二区精品久久久| A级毛片高清视频| 91精品国产剧情欧美一区二区| 国产品无码一区二区三区在线| 婷婷激情五月天四房| 爆操大奶子美女视频| 小穴抽插流水视频| 黑人巨茎和中国美女视频| 瓯美在线免费视频笫一区第二区| 色欲精品一区二区三区AV| 国产合区在线一区二区三区| 奇米一区二区三区视频在线观看| 成人刺激性视频在线观看| 一个色综合色综合色综合| 少妇毛片一区二区三区免费视频| 日本一区二区三区四区五| 人人摸人 人干人人草操|