TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

????????

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

???????????? ??

???? ???? ??? ???????? ???? ???? ?????. ?????? ?????? ??????? ??? *

视频一区视频二区制服丝袜| 日韩有码视频在线| 2021最新热播国产一区二区| 影音先锋亚洲中文综合网| 多男用舌头伺候一女| 国语自产免费精品视频在| 国产精品操大屁股老淑女| 精品国产自在久国产应用| 三级片手机在线视频| 极品 操 抽插视频| 男生鸡鸡插进女生笑穴里| 非洲人粗大长硬配种视频| 精品无码国产一区二区三区A| 大鸡巴操大屁股美女视频| 成人国产亚洲精品一区二| 色熟妇人妻久久中文字幕| 日韩中文字幕一区二区高清| 日韩人妻精品一区二区三区| 无遮挡粉嫩久久久久久久| 男女真人牲交高潮全过程| 亚洲欧美日韩另类| 午夜性刺激在线视频免费| 中国女人日逼免费片| 99爱这里只有精品| 中国美女操逼的视频| 视频一区视频二区制服丝袜| 欧美男女舔逼舔鸡巴视频| 男人把昆吧放女人屁股里| 强奷很舒服好爽好爽| 国产精品熟女一区二区三区久久夜| 欲色欲香天天网综合久久| 裸体午夜一级视频| 老色鬼精品视频二区三区| 好想大鸡巴插进阴道视频| 中文字幕乱码一区二区三区麻豆| 两人爽爽爽无码免费视频| 日韩欧美一区二区三区在线视频| 久久久久人妻一区精品加勒比| 视频一区二区三区日韩视频| 公交车上被后入搞逼漫画| 一区二区国产精品免费视频|