Non metallic inclusions mainly come from various types of non-metallic inclusion compounds formed by the corresponding increase of the equilibrium constants of oxygen, sulfur and nitrogen compounds in the process of liquid steel condensation. The products formed by chemical reaction should be called non-metallic inclusion or inclusion for short. Although the amount of inclusions in steel is small, it has a bad effect on the quality of steel materials and products. With the development of modern material engineering technology, the requirement of steel quality is increasingly strict. Therefore, in-depth study of non-metallic inclusions will be of great significance to material identification, product fracture analysis, scrap analysis and failure analysis.

1.Sources of non-metallic inclusions in steel

Inclusions are mainly caused by a series of physical and chemical reactions during melting and solidification of steel. According to their sources, they can be divided into endogenous (internal) inclusions and exogenous (external) inclusions.

endogenous inclusions

Endogenetic inclusions refer to the products produced by the chemical reaction between various material components in the process of steel smelting, casting and condensation, or the contact between the steel and the atmosphere or container in the furnace, or the particles precipitated due to the decrease of solubility when the condensation temperature of liquid steel decreases.

foreign inclusions

Foreign inclusion is also called external inclusion or accidental inclusion. It is due to the smelting, casting production process, from the equipment or container off and mixed into the liquid steel impurities. In addition, sometimes due to the negligence of smelting operation, the refractory brick cracks and falls off due to thermal impact, forming products with other kinds of oxides and becoming foreign inclusion

Non Metallic Inclusions in Steel and Methods to Identify Them 2

2.Influence of inclusions on steel quality

The harmfulness of inclusions depends on their quantity, shape, size, distribution, melting point, physical and chemical properties. When the inclusion has the property of low melting point, the steel will produce hot brittleness and crack due to its melting or softening during hot working. When there are aluminum inclusions or other nitrides in the steel, the surface hardness of the steel is not uniform, which makes it difficult to cut and grind. When the inclusion in the steel has exceeded the standard, it will bring great difficulties to the heat treatment and welding process, such as the uneven infiltration layer in the chemical heat treatment, and the strength of the weldment will be greatly reduced or cracked during welding

3.Metallographic identification of inclusions

Metallographic identification method can not identify the chemical composition and crystal structure of inclusions, but can directly observe and identify the shape, size, quantity, distribution and type of inclusions under optical metallographic microscope. At the same time, metallographic identification method also has the characteristics of simple operation and easy implementation.

interception and preparation of metallographic samples in order to ensure that the intercepted samples can represent the results of identification of non-metallic inclusions, the intercepted parts shall meet the requirements of corresponding technical conditions. For forging blank, samples can be taken from different parts from the center to the edge of forging blank, such as the head, middle and tail of forging blank; for rolled and cold drawn steel, samples should be taken longitudinally through the center line; for quenching crack, forging crack, hot rolling, stamping and failure fatigue fracture, samples should be taken at the crack and fracture; for special steel or product parts, samples can be taken according to the requirements It should be carried out according to the standard of the company.

The metallographic sandpaper from coarse to fine shall be used in the grinding process of the sample. The next grinding process shall be perpendicular to the grinding mark of the previous grinding process until the grinding mark disappears. In the polishing process, the polishing surface of the sample should be moved back and forth at the radius of the polishing disc with appropriate pressure, and the sample itself should also be rotated continuously. The final requirement is that the sample is not etched in 100 times field of view, and its surface has no scratch, no peeling, no water mark, no stain, smooth and bright as a mirror.

4. types and morphology of inclusions

Sulfides have high ductility, single gray inclusions with a wide range of shape ratio (length / width), generally with rounded ends; most of alumina have no deformation, with small shape ratio (generally < 3), and black or blue particles are arranged in a row along the rolling direction (at least three particles); silicate has high ductility, with a wide range of shape ratio Single black or dark gray inclusions (generally ≥ 3), generally with acute angle at the end; spherical oxides are non deformable, angular or round, small in shape (generally < 3), black or blue, irregularly distributed particles; single particle spherical inclusions are round or nearly round, diameter ≥ 13 μ M.

Non Metallic Inclusions in Steel and Methods to Identify Them 3
亚洲丁香婷婷久久一区| 翘臀少妇成人一区二区| 少妇淫真视频一区二区| 日韩精品一区二区三区射精| 国产精品日韩欧美第一页| 亚洲日本韩国一区二区三区| 欧美日韩亚洲国产综合网| 大香蕉久久精品一区二区字幕| 色综合久久超碰色婷婷| 日本一二三区不卡免费| 午夜视频免费观看成人| 九九热精品视频免费观看| 欧美黑人精品一区二区在线| 日韩精品中文字幕在线视频| 亚洲国产精品一区二区毛片| 麻豆亚州无矿码专区视频| 日韩一区二区三区免费av| 日本婷婷色大香蕉视频在线观看| 91人妻人人做人碰人人九色| 国产午夜福利片在线观看| 欧美野外在线刺激在线观看| 国产女高清在线看免费观看| 国产精品免费视频视频| 国产一区二区三区色噜噜| 国产人妻熟女高跟丝袜| 日韩一区二区三区18| 丰满人妻少妇精品一区二区三区| 99久久精品视频一区二区| 欧美日韩亚洲国产综合网| 日本在线高清精品人妻| 精品丝袜一区二区三区性色| 日本人妻熟女一区二区三区| 日韩一本不卡在线观看| 国产一区麻豆水好多高潮| 国产爆操白丝美女在线观看| 中文字幕一区二区三区大片| 视频在线播放你懂的一区| 日本中文在线不卡视频| 99福利一区二区视频| 日韩性生活片免费观看| 九九九热视频免费观看|