欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

Austenitic stainless steel has good corrosion resistance because of its high chromium content and dense oxide film. When Cr18% and Ni8% are contained, a single austenite structure can be obtained. Therefore, austenitic stainless steel has good corrosion resistance, plasticity, high temperature performance and welding performance. However, under different working conditions, austenitic stainless steel welding joints often face some special problems, which are easy to cause construction defects such as intergranular corrosion, stress corrosion, knife corrosion, welding hot cracks, α phase embrittlement and so on.

Corrosion analysis of welded joints

Intergranular corrosion of welded joints

Intergranular corrosion is one of the most important corrosion problems of austenitic stainless steel. Once intergranular corrosion occurs, its strength will almost lose when it is serious, and intergranular fracture will occur when a certain stress is applied. The intergranular corrosion of austenitic stainless steel welding joint is mainly caused by chromium carbide precipitation. When the austenitic stainless steel is sensitized in the temperature range of 500 ~ 800 ℃, the diffusion rate of supersaturated solid solution carbon to the intergranular boundary is faster than that of chromium, and the carbon in supersaturated solid solution is combined with chromium near the grain boundary, When the chromium content in the region is reduced to below the limit content (w (CR) 12.5%) required for passivation, the corrosion of the region will be accelerated and intergranular corrosion will be formed. The results show that the intergranular corrosion in the sensitized temperature zone of HAZ occurs in the region where the peak heating temperature is between 600 ℃ and 1000 ℃. The reason for intergranular corrosion is still the precipitation of chromium carbide at austenite grain boundary. The main preventive measures to reduce and prevent intergranular corrosion include:

① Small specification (small current, high welding speed) and multi pass welding are adopted;

② The carbon content in the base metal and welding material should be reduced as much as possible, and the welding material with C content less than 0.03% should be used;

③ As a result, Cr diffuses to the grain boundary more quickly in ferrite than in austenite, which reduces the phenomenon of poor chromium in austenite grain boundary;

④ The addition of Ti, Nb and other elements with stronger affinity to carbon than chromium in steel and welding materials can form stable compounds with carbon bonding, thus avoiding chromium depletion at austenite grain boundaries.

Stress corrosion of welded joints

The stress corrosion cracking of stainless steel is the most harmful corrosion behavior. There is no deformation when cracking. The accident is often sudden and the consequences are serious. There are many factors influencing the stress corrosion cracking of stainless steel under service conditions, including the composition, structure and state of the steel, the type of medium, temperature, concentration, stress properties, size and structural characteristics.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 2

The main measures to reduce and prevent stress corrosion are as follows:

① Avoid strong assembly, mechanical impact and arc burn, reduce cold work deformation and stress;

② Strictly control impurities in media and environment (especially chloride, fluoride, etc.);

③ Reasonable material selection (base metal, welding material): avoid grain coarsening and hardening martensite structure;

④ The weld is well formed without any stress concentration (such as undercut);

⑤ Arrange welding sequence reasonably to reduce stress;

⑥ Anti corrosion treatment: add corrosion inhibitor to coating, lining or cathodic protection.

 

Hot crack sensitivity analysis of welded joints

The hot cracks of austenitic stainless steel are mainly crystalline cracks, which are produced during the solidification process of liquid metal of weld metal. At this time, primary crystals exist in eutectic melting point, mainly between dendrites. The main reasons are as follows:

① S, P, C and so on form low melting point eutectic with Ni (for example, the melting point of NIS + Ni is 644 ℃), which weakens the grain boundary strength;

② Austenitic stainless steel has the advantages of large distance between liquidus and solidus, long crystallization time, strong dendrite orientation and easy to produce segregation of impurity elements;

③ The thermal conductivity of steel is small, and the linear expansion coefficient is large, so it is easy to produce stress.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 3

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 4 

The main measures to prevent welding hot cracks include:

① The contents of harmful impurities sulfur and phosphorus in base metal and welding material shall be strictly controlled;

② About 5% ferrite is produced in the weld, which disturbs the direction of austenite columnar crystal;

③ Small current and fast welding process are adopted.

Control of ferrite content in welded joints

The content of ferrite in weld metal of austenitic steel is not only related to the formation and thermal strength of α (σ) phase embrittlement, but also directly affects the hot cracking resistance of joint. The longer the heating time, the longer the high temperature residence time, the more precipitation, which will seriously affect the mechanical properties of the joint. From the point of view of hot cracking resistance, a certain amount of ferrite is required in the weld metal. However, considering the α phase embrittlement and thermal strength, the lower the ferrite content is, the better. Therefore, the content of ferrite must be strictly controlled for high temperature strength welded joints. In some cases, austenitic weld metal must be used.

Main Problems Encountered in Welding of 18cr Austenitic Stainless Steel 5

国产成人精品在线播放| 狠狠做深爱婷婷久久综合| 少妇毛片一区二区三区| 久久香蕉综合网精品视频| 久久婷婷综合色拍亚洲| 日韩性生活视频免费在线观看| 中文字幕日韩一区二区不卡| 午夜视频免费观看成人| 日韩中文字幕有码午夜美女| 国产精品国三级国产专不卡| 国产亚洲欧美自拍中文自拍| 日韩中文字幕视频在线高清版| 中文字幕免费观看亚洲视频| 午夜福利在线观看免费| 国产精品成人免费精品自在线观看| 国产肥女老熟女激情视频一区| 美女被草的视频在线观看| 亚洲最大福利在线观看| 欧美大胆女人的大胆人体| 亚洲精品中文字幕一二三| 亚洲一级在线免费观看| 精品香蕉国产一区二区三区| 91欧美日韩精品在线| 又黄又硬又爽又色的视频| 国产精品久久精品国产| 加勒比人妻精品一区二区| 黑人粗大一区二区三区| 午夜资源在线观看免费高清| 欧美一区二区在线日韩| 日韩一区二区三区观看| 欧美日韩中黄片免费看| 欧美熟妇喷浆一区二区| 欧美中文字幕一区在线| 夫妻性生活动态图视频| 亚洲深夜精品福利一区| 91精品欧美综合在ⅹ| 日韩18一区二区三区| 日本不卡在线视频你懂的| 中文字幕日韩精品人一妻| 欧美激情区一区二区三区| 亚洲天堂精品1024|