欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

As with traditional machining methods, EDM machining of cemented carbide will cause carbide cracks initiation as well, but engineers often ignore this fact because WEDM is high-precision machining. We often use WEDM to process cemented carbide products that are small in size, complex in shape and cannot be processed by grinding wheel. However, engineers generally take dimensional accuracy, surface roughness and production efficiency into consideration while ignore the influence of WEDM on the micro-structure area of the carbide surface.

 

Carbide crack initiation mechanism

Different from general machining, the wire cutting wire doesn’t contact the work piece directly, but gradually erodes the metal material by the continuous pulse spark discharge generated between them. In WEDM, the temperature of the machined surface changes rapidly and lead to uneven stress on work piece. This situation is particularly at ease to occur in the processing of hard and brittle materials, such as cemented carbide, cermets, etc. In past empirical research ,When the electrical parameters are not set up properly, crack initiation will appear on the surface of the work piece once the thermal stress exceeds the strength limit.

pic of how wedm working on carbide and produce carbide initiation

According to the thermal stress model, the amount of heat entering the material is proportional to the peak stress. This heat is directly related to the input electric pulse energy under the same other conditions, which is that the greater the input power, the more heat the material absorbs and the greater the stress. Under the condition of neglecting the energy loss, the energy acting on the workpiece during processing can be simplified as below,

3 Facteurs importants qui provoquent l'initiation de la fissure du carbure du produit en carbure dans WEDM 1

In this formula, W is the pulse energy (J); U is the intermittent instantaneous discharge voltage (V); I is intermittent instantaneous discharge current (A); T is the time (s); Tk is the discharge duration (pulse width, s).

In this formula, W is the pulse energy (J).U is the intermittent instantaneous discharge voltage (V).I is intermittent instantaneous discharge current (A).T is the time (s). Tk is the discharge duration (pulse width, s).

It can be seen from the formula that when the discharge duration (pulse width) is determined, increasing the discharge voltage and current will aggravate the crack initiation. When the discharge voltage and current are determined, increasing the discharge duration (pulse width) will result in the same outcome.

 

Experiment plant of micro crack initiation on carbide

A bunch of cemented carbide bushings (see Figure 2) ,made of YG6 cemented carbide (Chinese carbide grade), will be processed for the experiment. ?The bushing’s in height of 30mm, with key slots in width of 1.6mm and depth of 1mm. After being processed, the bushings will be made into metallography sample for SEM inspection to observe the crack initiation and propagation on the machined surface of cemented carbide。

3 Facteurs importants pour l'initiation de la fissure du carbure du produit en carbure dans WEDM 2

In the test, the medium wire cutting equipment CTP350 is used. The cutting fluid is emulsion with a concentration of 8%, and the cutting wire is φ 0.18mm molybdenum wire, one piece is clamped at a time for processing, and the processing parameters of wire cutting are shown in Table 1.

Other main test condition:
edm machine: CTP350
cooling fluid: 8% emulsion
cutting wire:φ0.18 molybdenum wire
processing times limit: 1 piece a time
and WEDM processing set-up parameters are shown in the following table 1.

3 Facteurs importants provoquant l'initiation de la fissure de carbure du produit de carbure dans WEDM 3

The test result about WEDM carbide crack initiation involving 4 factors

Electricity pulse width

Metallographic photos of 1 #~4 # products are shown in Fig. 3~Fig. 6. It can be seen from the figure that with the decrease of pulse width, the microcracks on the alloy surface gradually become smaller. When the pulse width is 40ms, the depth of microcrack reaches mmmm; When the pulse width is 12 ms, there is basically no crack initiation.

3 Facteurs importants provoquant l'initiation de la fissure de carbure du produit de carbure dans WEDM 4

Electricity current value

The metallographic photos of 5 #~8 # products are shown in Fig. 7~Fig. 10. It can be seen that when the processing current is 3.5A, the crack depth is more than 30mm; When the processing current is 2.8A, the crack depth is 30mm; When the processing current is 2.4A, the crack depth is 20mm; While the processing current is 2.0A, the crack depth is 10mm. All in all, the greater the machining current, the greater the crack depth.

3 Facteurs importants provoquant l'initiation de la fissure de carbure du produit de carbure dans WEDM 5

Voltage

The metallographic photos of product 9# ~ 12# are shown in Figure 11 ~ 14.?It can be seen that when the current is 2A, the pulse width is 20μm, and the pulse interval is 8 times the pulse width, the processing voltage is 70 ~ 120V, and no alloy microcracks are found in the cutting section. In other words, the influence of voltage on the carbide crack?initiation?is not obvious when the current and pulse width are constant.

3 Facteurs importants provoquant l'initiation de la fissure de carbure du produit de carbure dans WEDM 6

Cutting times

The metallographic photos of 13 #~15 # products are shown in Figures 15~17. It can be seen that through multiple cutting processes, the surface quality of the product become better and micro-crack’s depth gradually reduced as cutting times grow. The depth of the micro-crack of the product is within 15mm after two times of WEDM processing; The depth of micro-cracks in the product is within 10mm after three times of WEDM processing. Thus, through two times of cutting processing, it can meet the requirement that the micro-crack depth of carbide bushing should be less than 20mm.

3 Facteurs importants provoquant l'initiation de la fissure de carbure du produit de carbure dans WEDM 7

The experimental summary of cracks in cemented carbide produced by WEDM

When WEDM is used to process brittle materials such as cemented carbide, the pulse width and processing current have obvious effects on the microcracks on the surface of the alloy, which are shown in the following aspects: the greater the pulse width and current, the deeper the crack. However, the effect of voltage on the surface microcracks of the alloy is not obvious. No microcracks were found when the pulse width was 12 μm.

When the working current is above 2A, the workpiece will have cracks to a certain extent. Therefore, when selecting electrical parameters, avoid selecting the processing current above 2A. The superposition effect of temperature field should be fully used to reduce the size of thermal stress and its impact property, so that the workpiece material can be thrown out in gas phase to avoid overheating of the workpiece surface.

In addition, multiple cutting is a very effective method to reduce and remove surface microcracks.

Laisser un commentaire

Votre adresse de messagerie ne sera pas publiée. Les champs obligatoires sont indiqués avec *

一区二中文字幕在线看国产一区| 国产一级第一级毛片| 男人扒开女人腿狂躁免费| 欧美一区二区三区四区五区精品| 插逼爽歪歪视频免费| 欧美黄色三级成人小视频| 亚洲一区二区女同性恋免费看| 精品日本一区二区三区视频播放| 久久一级高潮a免费| 国产无圣光一区福利二区| 欧美大鸡巴捅骚逼吃| 亚洲欧美日韩中文v在线| 黄网官方在线观看| 精品的极品美女一区二区三区| 久久久国产系列丝袜熟女| 久久久久亚洲精品无码系列| 亚洲一区二区女同性恋免费看| 两人爽爽爽无码免费视频| aaa啊啊啊黄片| 好爽轻点太大了太深了视频| 插女人下面高潮视频| 97人妻精品一区二区三区视频| 日韩av一区二区三区激情在线| 亚洲欧美日韩精品一区二区| 大香蕉中码手机在线视频| 中文无码av动作片| 亚洲综合极品香蕉久久网| 中文字幕在线资源第一页| 色偷偷影音先锋男人av| 无码中文字幕免费一区二区三区| 国产亚洲精品一区久久| 香蕉国产精品偷在线| 男人透女人视频短篇| 日本不卡高清视频在线播放| 午夜理论理论亚洲激情| 欧美精品日韩精品中文字幕| 中文字幕乱码人妻一区二区三区| 色噜噜在线一区二区三区| 国产天美传媒剧免费观看| 三级片手机在线视频| 爱爰哦好粗好猛操b视频|