The size of WC grains is of great significance to the friction and wear properties of cemented carbide. It is generally believed that coarse-grained cemented carbide has poorer wear resistance than fine-grained cemented carbide. After the grain refinement of cemented carbide, the size of the hard phase decreases, increasing the surface area of the hard phase grains and the bonding force between the grains, and the binder phase is more evenly distributed around them, which can improve the hardness and wear resistance of the cemented carbide. In this paper, the author conducts friction and wear experiments on cemented carbide to analyze the friction and wear properties under different parameters and the material removal mechanism, providing experimental evidence for the optimization design of high-speed cutting tool materials, reasonable material selection, and the study of high-speed cutting wear mechanisms.

Experiment

Test Materials

Three types of WC-6Co cemented carbide with different grain sizes were selected for the test. The size of the cemented carbide disc was φ55mm×4mm, and the surface was rough ground, finely ground, and polished. The mating material used was Al?O? balls with a diameter of 9.5mm. Both samples were ultrasonically cleaned in acetone for 20 minutes and dried for use. The material properties are shown in Table 1.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 2

Friction and Wear Test

The test was conducted on a UMT-2 multi-functional friction and wear testing machine produced by CETR Corporation in the United States, using a ball-on-disc contact method. The structure of the testing machine is shown in Figure 1. The cemented carbide friction disc was attached to the working table with double-sided tape, and the Al?O? ball was placed in the fixture. The two types of mating materials produced mutual movement and force of action. The friction force generated was detected by the sensor, and the curves of friction force, normal force, and friction coefficient were automatically generated by the related software according to Coulomb’s law.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 3

The test was conducted at room temperature, with normal forces of 10N and 20N respectively, and the linear velocities of the friction pair sliding were 40m/min, 80m/min, 120m/min, and 160m/min. The sliding distance was 500m. After the test, a scanning electron microscope (SEM) was used to observe the wear scar surface morphology of the upper and lower samples, and an X-ray energy dispersive spectrometer (EDS) was used to detect the elemental composition of the worn surfaces. All samples were analyzed for the elemental composition of the friction and wear surfaces under the same conditions.

Results and Analysis

Friction and Wear Performance

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 4

Figure 2 shows the friction coefficient curve of ZH cemented carbide drawn by the testing machine’s accompanying software (load 20N, sliding speed 160m/min). The experiment found that each friction process follows a similar pattern, that is, the initial dynamic friction coefficient undergoes a rapid increase from the initial value during the transition period, and then remains relatively stable, showing a fluctuating characteristic in the stable phase. In the beginning, under the action of the normal load, only local micro-convex bodies on the friction surface are in contact, the adhesive area is small, and the molecular attraction on the contact surface is weak, so the friction coefficient is small; as the friction process progresses, the micro-convex bodies interfere with each other, gradually get worn down, the adhesive area increases, and the molecular attraction also increases, leading to a gradual increase in the friction coefficient. The entire friction process is a continuous process of the contact surface adhering and then being sheared under the action of shear stress. Due to the peeling and breaking of the Co phase on the surface, the wear of the sample surface occurs, and the local adhesion on the surface quickly reaches a dynamic equilibrium, resulting in the friction coefficient of the surface being maintained within a relatively stable range, which is called the stable period.

Most scholars use the average value of the friction coefficient over a period of time (distance) as a characterization parameter of friction behavior. Therefore, this experiment selects the average value during the stable friction phase as the friction coefficient of the cemented carbide under the corresponding parameters. Figure 3 shows the friction coefficients of three types of cemented carbide under different loads and speeds.

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 5

It can be seen that with the increase of friction speed and load, the friction coefficient of the cemented carbide generally shows a decreasing trend, and the decrease is most obvious in the transition from relatively low speed (40m/min and 80m/min) to high speed (120m/min and 160m/min). From the perspective of material, the friction coefficient of ZH cemented carbide is smaller than that of the other two materials, and the friction coefficients of ZHX and HG cemented carbides are not significantly different, with the friction coefficient of HG cemented carbide being slightly larger.

Wear Mechanism

After the friction and wear tests, the microstructure of the worn surfaces of each sample was observed using a scanning electron microscope (SEM), and SEM images were taken, along with an analysis of the surface composition. The friction and wear mechanisms of the cemented carbide under different friction parameters are similar, as shown in Figure 4 (sliding speed 160m/min, load 20N).

How Grain Size Transforms Cemented Carbide's Friction and Wear Performance 6

In the initial stage of cemented carbide wear, the binder phase Co undergoes plastic deformation, and the surface layer of Co is extruded by the WC grains. Due to the low hardness and good ductility of Co, under certain conditions, a micron-scale friction film can form on the surface, while the harder WC particles gradually protrude from the friction surface, preventing further rapid wear of the surface and allowing the friction process to enter a relatively stable stage. As the binder phase Co continues to be lost, the WC framework of the material is damaged, and the dislocation density within the WC particles significantly increases. When the dislocation density accumulates to a certain extent, microcracks will form on the WC particles, causing the WC particles to begin to pull out from the cemented carbide matrix. The detached WC particles remain in the wear area, transforming into abrasive particles, which, under the action of the load, compress against the matrix, resulting in new plastic deformation and grain damage.

cemented carbide

As can be seen from Figure 4, as the grain size of the cemented carbide decreases, the grain density increases, and the degree of surface wear decreases. The surface of the ZHX cemented carbide shows no obvious shedding of WC particles, while the surface density of HG is very good, with almost no obvious shedding of WC particles. Therefore, for the traditional grain size cemented carbide ZH, the main wear mechanism is abrasive wear caused by the extrusion of the binder phase Co and the shedding of WC grains. As the grain size decreases and the density of the fine-grained cemented carbide increases, the phenomenon of WC grain spalling decreases, Co still wraps around the WC, the microstructure of the material remains intact, and most grains only undergo a certain degree of plastic deformation.

Conclusión

The size of WC grains has an important effect on the friction and wear properties of cemented carbide. As the grain size decreases, the friction coefficient slightly increases, and the wear resistance is enhanced.

The friction coefficient of cemented carbide is influenced by speed and load, and it shows a decreasing trend with the increase of speed and load.

The wear mechanism of traditional grain size cemented carbide is mainly characterized by the extrusion of the binder phase Co and the fracture and spalling of the hard phase WC grains; the grain spalling phenomenon of fine-grained cemented carbide is not obvious, and the main wear mechanism is plastic deformation.

Deja una respuesta

Tu dirección de correo electrónico no será publicada. Los campos obligatorios están marcados con *

大香蕉中码手机在线视频| 白虎美女被大基吧操| 黑人大屌大战中国女| 日韩伦理视频一区二区三区| 中文字幕欧美中日韩精品| 国产青青操骚货在线观看| 国产一区精品在线| 东京热无码AV一区二区三区| 久久一区二区三区精华液介绍| 国产一级第一级毛片| 久久精品国产自清天天线| 黄片大鸡吧操小逼| 束缚久久久久久免费高潮| 两个人免费视频高清| 午夜成人理论片在线观看| 精品久久久久五月婷五月| 两个人免费视频高清| 精品少妇一区二区三区中文字幕| 国产激情内射免费精品| 爽妇网国产精品24| 精品一区二区久久久久无码| 极品美女销魂一区二区三区| 精品久久久久五月婷五月| 女人被躁到高潮嗷嗷叫小| 插我舔内射18免费视频| 午夜成人理论片在线观看| 国产亚洲一区二区手机在线观看| 国产精品一区二区日本欧美| 男人扒开女人腿狂躁免费| 成人高清在线播放一区二区三区| 加勒比在线不卡一区二区观看| 大黑屌后入骚妇屁股| 大肉棒操小骚穴视频| 熟女菊蕾老妇俱乐部视频| 精品久久久久五月婷五月| 色橹橹欧美在线观看视频高清免费| 黑人巨茎和中国美女视频| 操你的骚逼粉嫩AV| 国产精品你懂的在线资源| 天美传媒精品1区2区3区| 日韩午夜资源在线观看|