Machining titanium alloy is hard because the thermal conductivity of titanium alloy is very poor. Coupled with the short contact length between the chip and the cutting tool, it is not conducive to the dissipation of cutting heat. As a result, the temperature in the cutting edge region is high, about more than twice that of cutting 45 steel. In addition, tool wear is also severe. On the one hand, the strong chemical affinity between titanium alloy and tool material makes it easy to bond with elements such as Ti, Co, and C in the tool material, aggravating adhesive wear at high temperatures. On the other hand, titanium alloy easily forms a hard and brittle surface layer by reacting with oxygen and nitrogen in the air, exacerbating tool wear.

Table 1: Selection of Tool Geometric Parameters for Turning Titanium Alloys

Tool material Front Rake Angle ?Back Rake Angle Cutting Edge Inclination Angle Main Clearance Angle Secondary Clearance Angle Chamfer Width (mm) Chamfer Front Angle Cutting Edge Radius (mm)
Carbide lathe 5~10 10~15 0~10 45~75 15 0.05~0.3 0.10~0 0.5~1.5

What are the Challenges in Machining Titanium Alloys? 1

Machining amount

The cutting speed for turning titanium alloys should not be too high, and the cutting depth can be relatively large, while the feed rate should be appropriate. A feed rate that is too large can cause burning of the cutting edge, while a feed rate that is too small results in rapid wear of the cutting edge when processing the hardened layer. When turning titanium alloys, rust-proof emulsion or extreme-pressure emulsion can be used for cooling and lubrication. The recommended cutting parameters for turning titanium alloys are as shown in

Table 2: Selection of Cutting Parameters for Turning Titanium Alloys

Feed (mm) cutting speed(mm)
0.08~0.12 87~69
0.13~0.17 71~59
0.16~0.24 62~51
0.25~0.30 53~47
0.33~0.44 48~41
0.45~0.65 42~34

Note: Conditions for the use of this table: Tool material YG8, workpiece material TC4, tool geometric angles front rake angle = 5°, back rake angle = 10°, main clearance angle = 75°, secondary clearance angle = 15°, cutting edge radius = 0.5mm, turning depth = 1mm, dry turning. If using cutting fluid, the turning speed in the table can be appropriately increased.

What are the Challenges in Machining Titanium Alloys? 2

Machining parameters

Machining Temp.

When turning titanium alloys, the cutting temperature is high, and tool durability is low. Among the cutting parameters, cutting speed has the most significant impact on cutting temperature. Therefore, efforts should be made to ensure that the cutting temperature generated at the selected cutting speed is within the optimal range. The recommended cutting temperature for turning titanium alloys with high-speed steel tools is approximately 480°C to 540°C, while for hard alloy tools, it is around 650°C to 750°C.

Cutting speed Vc

The cutting speed has the most significant impact on tool durability, and it is preferable to operate the tool at the optimal cutting speed with minimal relative wear. When turning titanium alloys of different grades, the cutting speed should be adjusted appropriately due to significant differences in strength. The turning depth also has a certain influence on the cutting speed, and the magnitude of the cutting speed should be determined based on different turning depths.

Feed rate

The feed rate has a relatively small impact on tool durability. While ensuring the machining surface roughness, a larger feed rate can be chosen, typically ranging from f=0.1 to 0.3 mm/r. If the feed rate is too small, the tool may cut within the hardened layer, increasing tool wear. Additionally, extremely thin chips are prone to spontaneous combustion at high cutting temperatures, so a feed rate below f<0.05 mm/r is not allowed.

Cutting depth (ap) has the least impact on tool durability. A larger cutting depth is generally chosen to avoid cutting within the hardened layer, reducing tool wear. It also increases the working length of the cutting edge, promoting heat dissipation. Typically, ap is set at 1 to 5 mm.

Schreibe einen Kommentar

Deine E-Mail-Adresse wird nicht ver?ffentlicht. Erforderliche Felder sind mit * markiert.

一区二中文字幕在线看国产一区| 99热这里只有精品亚洲| 成人 在线 欧美 日韩| 国产日女人视频在线观看| 男人几把操女人嫩穴| 中文字幕一区二区日韩精品蜜臂| 99热这里只有精品98| 那种视频在线观看你懂的| 美女骚逼黄色18禁| 亚洲精品自拍偷拍第一页| 国产一二三四五自产| 亚洲一区亚洲二区在线观看| 亚洲欧美中文字幕第二十| 日韩亚洲AV无码一区二区不卡| 草草久性色av综合av| 久久99国产中文| 大鸡扒干美女BB直流水| 国产成人AV一区二区在线观看| 黄色日女人逼视频| 熟妇女人妻丰满中文字幕| 美女被操的流水AV| 99精品欧美一区二区三区喷胶| 狠狠五月激情综合去干网| 99久久久国产精品美女| 无遮挡粉嫩久久久久久久| 干女人逼逼的大几把| 亚洲国产精品伦理在线看| 下载风骚美女想吃大机吧| 高颜值美女视频在线观看| 91kaobi视频在线| 啊啊啊好疼视频进来| 国产 自拍 欧美 在线| 久久综合日韩亚洲精品色| 大黑屌爆操日本女人| 亚洲男性天堂一区二区三区| 亚洲男人的天堂2023| 中文国产成人精品久久久| 中文有码无码人妻在线看| 欧美办公室大鸡巴| 粗大长内射女人视频| 啊灬啊别停灬用力啊男男在线观看|