Due to the “dual high” characteristics of high hardness and high toughness, the application scope of ultrafine-grained carbides has been expanding, leading to the development of tungsten carbide (WC), the main raw material for carbides, towards ultrafine particles. This is an undeniable fact. However, coarse-grained WC?possesses a series of advantages such as fewer microstructural defects, high microhardness, and low microscopic strain. As a result, it finds extensive applications in mining tools, petroleum drilling tools, engineering machinery, stamping dies, and hard surfacing technologies. In particular, its application in hard surfacing technology has rapidly developed in recent years, such as the production of pipe-type welding rods, electrodes, and spray welding powders using coarse-grained WC. Coarse-grained WC has been identified as a cost-effective wear-resistant hard surfacing material, which is of great significance in improving the efficiency of mechanical equipment and conserving metal materials.

The traditional method for producing coarse-grained WC?involves the following steps: WO? is reduced at high temperature to obtain coarse tungsten powder, which is then subjected to high-temperature carburization to produce coarse-grained WC. The WC produced by this process is approximately 22μm in size. This method has dominated the domestic industry for a long time.

How to Manufacture Coarse-Grained WC Using Activated Additive Method 2

Development of Production Methods

In the past decade, there have been continuous updates in the manufacturing methods of coarse-grained WC?powder, including:

method 1 for coarse-grained WC Powder

High-temperature carburization of medium or fine tungsten powder: This process can produce coarse WC grains with a particle size of 7-8μm.

method 2

MACEO (Microplasma-Assisted Chemical Etching of Oxygen) method: This process can produce extremely coarse WC powder with a sieve size larger than 40 mesh. However, it requires special treatment and impurity purification before being used for manufacturing carbides.

method 3

Cobalt-nickel carburization method: This process utilizes a small amount of cobalt and nickel to accelerate the carbide formation of tungsten particles and promote rapid growth of WC grains. With this mechanism, coarse-grained WC with a particle size of 22μm can be produced at relatively low temperatures.

method 4

Classification of coarse-grained WC powder: This method involves using techniques such as cyclone separation, fluidized bed classification, liquid elutriation, or sieving to separate large particles containing W?C and free carbon from WC. This not only narrows the particle size distribution range but also improves the quality of WC powder by increasing the compound carbon content and reducing the free carbon content.

As the application scope of coarse-grained WC?continues to expand, the demand for coarse carbide with a particle size larger than 22μm cannot be met. Therefore, it becomes necessary to develop new coarse-grained WC?products with a particle size greater than 30μm. After several years of exploration, we have successfully experimented with the additive method to produce coarse-grained WC?powder with a particle size larger than 30μm. This method has the advantages of a simple and feasible process, easy operation, utilization of existing production lines without the need for additional equipment, low process temperatures that save energy and prolong the lifespan of process equipment, and high purity of the produced product with no residual additives. The particle crystallization is intact, and the particle size distribution is uniform, consistent with the normal production of WC for carbides.

How to Manufacture Coarse-Grained WC Using Activated Additive Method 3

Experimental Method and Results

How to Manufacture Coarse-Grained WC Using Activated Additive Method 4

The experiment utilized blue tungsten oxide, produced by our factory, as the raw material. After uniformly adding the additive, it was subjected to continuous hydrogen reduction in a furnace at temperatures ranging from 900 to 1100°C, resulting in the production of tungsten powder (W). After carbonization with appropriate carbon content, the tungsten powder was further subjected to a one-hour carbonization process at around 2000°C in a continuous direct-heating carbon tube furnace. The coarse-grained WC?powder was obtained after ball milling and crushing.

The properties of the raw material, blue tungsten (W), are shown in Table 1. The properties of the intermediate product, tungsten powder (W), can be found in Table 2. The properties of the final product are presented in Table 3.

Using 1# WC with approximately 10% Co in the conventional process, the performance of the produced carbide?is as follows: strength of 2560 N/mm2, hardness of 86.5 (HRA), density of 14.42 g/cm3, magnetic flux density of 5300 A/m2, and WC grain size of 3.5 μm.

 

Analysis of Experimental Results

The above experimental results demonstrate that the additive used in the reduction and carbide formation processes of tungsten significantly increases the grain size of tungsten powder and tungsten carbide particles. As a result, various physical properties of tungsten powder and tungsten carbide powder undergo significant changes.

How to Manufacture Coarse-Grained WC Using Activated Additive Method 5

Compared to products without the additive, the addition of the additive can increase the particle size of tungsten powder by 3.5 to 4.5 times and the particle size of tungsten carbide powder by 2.5 to 3.0 times. Within the scope of the experiment, the process temperature has a significant influence on the particle size of tungsten powder and tungsten carbide. However, the variation in additive content does not have a significant impact on the particle size of tungsten powder and tungsten carbide powder.

coarse-grained WC

Preliminary Exploration of Activation Mechanism

The experimental results indicate that the additive promotes the growth of WC particles, mainly during the tungsten reduction stage. However, during the carbide formation process, the particle size of the product does not increase and, in fact, slightly decreases.

It is well known that the reduction of blue tungsten (primarily composed of WO?go) to tungsten powder undergoes several stages: WO?go → WO?n → WO? → W. During the WO?go → WO? stages, the product generally maintains the particle morphology of its precursor. However, during the WO? → W stage, almost all particles undergo a significant change in morphology and there is a considerable variation in particle size. This can be attributed to two main reasons: first, the solid-state phase transformation during the reduction process leads to particle fracture and refinement; second, the volatilization → reduction → deposition mechanism causes particle coarsening.

How to Manufacture Coarse-Grained WC Using Activated Additive Method 6

 

We believe that the presence of the additive not only enhances the volatilization → reduction → deposition process by creating an additional channel for the formation of WOxnReO(gas), but also suppresses particle fracture during certain solid-state phase transformations that occur during the reduction process. This further exacerbates the coarsening and refinement of intermediate reduction products. As a result, the additive increases the base number of tungsten powder particles that undergo growth and intensifies the cycle of re-oxidation → volatilization → reduction → deposition of fine tungsten powder particles. This is the mechanism by which the additive activates and promotes the growth of tungsten powder particles during the reduction process.

 

Summary and Current Issues In this study

it is observed that the carbide process conditions for tungsten powder described in the paper are not entirely optimal. As a result, some of the coarse particles in the final product of WC powder contain W?C inclusions in their cores, accounting for approximately 2.4% of the total particles, as shown in Figure 1. Therefore, further improvements are required in the carbide process to ensure its suitability for the production of carbides.

 

 

 

 

Schreibe einen Kommentar

Deine E-Mail-Adresse wird nicht ver?ffentlicht. Erforderliche Felder sind mit * markiert.

操逼啊 啊 啊黄色视频| 久久久久人妻一区精品加勒比| 一区二区三区国产l精品欧美| 中文字幕av一区二区三区蜜桃| 92婷婷伊人久久精品一区二区| 哈啊慢点不要了视频| 国产成人亚洲精品在线看| 欧美大鸡巴插入骚b| 少妇精品久久久一区二区免费| 亚洲av一区二区在线看| 国产黄片在线免费看| 好嗨哟直播看片在线观看| 大鸡巴操饿罗斯女人| 中文字幕乱码一区三区免费| 老女人爱精大鸡吧草| 一级美女插逼百度| 东京热无码AV一区二区三区| 中文字幕精品字幕一区二区三区| 中国毛茸茸的操逼| 99久久国产综合精品女| 校花内射国产麻豆欧美一区| AV无码超清破解版流出| 乱伦美女小骚货视频| 狂插美女大屁股在线观看| 大粗鳮巴r教师人妻91| 日本男人捅女人机机| 国产精品毛片无遮挡高清| 亚洲午夜国产片在线观看| 麻豆视频一级片在线观看| 淫荡扣逼骚逼视频| 一色道久久88加勒比一| 黄色日女人逼视频| 亚洲av午夜一区二区| 日日狠狠久久888av| 亚洲精品一区二区精华液| 娇嫩的被两根粗大的np| 久久69精品久久久久免| 亚洲欧美日韩精品一区二区| 日本免费无码一区二区到五区| 久久久久久亚洲精品首页| 中国熟女色av夜夜嗨|