欧美人妻精品一区二区三区99,中文字幕日韩精品内射,精品国产综合成人亚洲区,久久香蕉国产线熟妇人妻

We used metallographic microanalysis and hardness testing methods to study the cause of the failure of cold-punching mould, and proposed an effective measure to improve the life of the mold. Research shows that by optimizing the heat treatment process and processing technology, the material selection is more reasonable and the service life of the mold can be greatly increased.The life of the cold-punching mould is the key factor that can cause the industrial production efficiency failing to improve. The factors that generally lead to die failure include early failures such as chippingand breaking, or serious deformation of the die and no further use. How to improve the die The service life has become a hot topic that the mold industry is highly concerned about.1 Types and Causes of Failure of Cold DiesAccording to the cause of the failure of the mold, the common failure modes can be divided into four failure modes: fracture failure, wear failure, deformation failure, and fatigue failure.Failure formReason for failureFailure failureMold material toughness and strength is not enoughWear failureExcessive wear due to relative motion between the mold and the material being groundDeformation failureMaterial heat treatment deformation, stress concentration, excessive load on the mold, plastic deformation of the materialFatigue failureCracks are continuously generated and expanded under alternating stressCold punching die usually work under difficult and complicated conditions, so die failure is often accompanied by multiple failure modes. Figure 1 starts to crack after stamping 800 pieces.It is made of Cr12MoV wear-resistant high-chromium alloy steel, the design hardness of 55 ~ 58HRC. The quenching process of the mold is (870℃x1.5h + 1050℃x2h) In a vacuum furnace, drawing fire 200℃x 3h. The measured hardness of the mold is shown in Table 2.Fig. 1 Mold partsTable 2 Mold Parts Hardness Test (HRC)Analysis: As can be seen from Table 2, there is a non-uniform distribution of the hardness of the mold parts, which is caused by the uneven heating of the mold during the heat treatment due to the large size of the mold parts. As shown in the metallographic organization chart of Figure 2, the material segregation of the mold parts is very serious due to the insufficient forging during the forging process. There was no macroscopic plastic deformation at the fracture surface and it was granular, and it was judged to be brittle fracture. Figure 2 Metallic microstructureMeasure: Metallographic examination of the metallurgical dimensions is less than 3 levels after full forging. Roughing high-temperature quenching and tempering treatments are added between finishing and finishing. 2 Measures to Improve the Life of Cold Dies 2.1 Reasonable Material SelectionWhen carbon alloy steel is used for brittle fracture due to insufficient plasticity, better tough materials such as microhardened steel 6CrMnNiMoVSi(GD), 9Mn2V steel, low alloy CrWMn steel, 7CrSiMnMoV(CH) steel should be selected. When wear failure is the main failure mode, alloy steels with high carbon content and chromium content (such as Cr12, Cr12MoV), high-carbon medium-chromium alloy steel (Cr8MoWV3Si), 9Cr6W3Mo2V2 (GM) steel, 7Cr7Mo2V2Si (LD) steel, etc. should be used.2.2 Heat Treatment Process ImprovementFirst of all, we must improve the pre-heat treatment process to refine the solid solution of carbides, improve the morphology and distribution of carbides, and increase the plasticity of workpieces. The second is to determine a reasonable quenching conditions, shorten the high-temperature residence time, rotate into the coolant and rotate it to seek even cooling, in order to avoid the failure of the mold.2.3 Reasonable forgingHigh-chromium alloy steels often have severe segregation of carbides and are forged using the cross-draft method. The carbide level after forging is not greater than grade 3. Strictly control the forging temperature and prevent the generation of forging cracks. After the forging, it is often used to anneal the residual heat balls and prepare for the final heat treatment.2.4 Wire cuttingThe size of the wire cutting processing power directly determines the white bright layer thickness and micro-cracks size of the quenched martensite formed on the surface of the workpiece. In the final step of in-line cutting, a small amount of energy is often used for finishing, which can greatly reduce the thickness of the bright white layer and the depth of cracks. After the wire cutting is completed, the mold should be supplemented and tempered to eliminate the additional stress of the wire cutting.3 ConclusionThe working conditions of cold working molds are relatively complex and bad. In the course of use, molds are often intertwined with various kinds of damage. Through the optimization of the heat treatment process and processing technology, the material selection is more reasonable and the service life of the mold can be effectively prolonged.
??????: Meeyou Carbide

???? ???????

?? ??? ??? ????? ????? ??????????. ?????? ????????? ???? ????? ?? *

国产精品国产三级国| 97超视频免费在线观看| 波多野吉衣吹潮Av| 二次元男生操女生屁眼爽| 99热这里只有精品97| 大鸡吧天天草黑逼| 一级毛片完整版免费播放一区| 欧美一区亚洲一区视频在线观看| 大胸瑟瑟黑丝午夜| 日本老熟妇毛茸茸| 高清无码精品一区二区三区| 美女扒开腿让男人桶爽揉| 丁香婷婷色婷婷粗大| 午夜精品福利一区二区三区蜜桃p| 护士毛片在线看中文字幕| 性一交一子一伦一乱| 春宵福利导航91| 美女麻豆颜色光屁股眼子| 插逼爽歪歪视频免费| 男生鸡鸡插进女生笑穴里| 一区二区三区亚洲av| 精彩欧美一区二区三区| 国产精品操大屁股老淑女| 狂插美女大屁股在线观看| 日本高清一区二区三区水蜜桃| 在线看免费无码a片视频| 国产成人AV剧情| 国产一级a不收费| 爆乳喷奶水无码正在播放| 国产成人AV一区二区在线观看| 国产高清第一区第二区第一页| 日韩一区二区三区国色天香| 胸大裸体美女视频| 精品精品视频国产| 我想看操小嫩逼大片| 中文字幕亚洲精品女同一页| 国产精品亚洲一区二区三区极品| 色男人天堂亚洲男人天堂| 色一情一交一乱一区二区| 国产精品人妇一区二区三区| 97超级免费视频在线观看|