TaC?carbide has been?one of the earliest carbide?put into industrial production?since traditional WC-Co carbides can no longer meet people’s demands for higher product quality. TaC is considered to improve the high-temperature performance of carbide. Meetyou Hardmetal Corp. conducted the following experiment, using WC with different particle sizes as the research object, and studying the properties of TaC tungsten carbide?sintered at different temperatures.

Experiment method

The formulation of the carbide?consists of w(Co)=6.0% and w(TaC)=1.85%. In the WC powder, the mass fraction of particles with an average Fechner size of 4.90μm is 44%, and the mass fraction of particles with a size of 0.89μm is 56%.

The ball-to-powder ratio is 4:1, and the mixture is wet-milled in ethanol at a speed of 50r/min for 65 hours in a 160mm diameter ball mill. Then, the powder is pressed into a B-type bar with dimensions of 20mm x 5.4mm x 6.5mm using a rubber processing procedure. The bars are sintered in a vacuum dewaxing furnace at 1425℃, 1450℃, and 1500℃ for 1.5 hours each.

Afterwards, our experimental staff analyzed the microstructure of the material using scanning electron microscopy, measured its density using an analytical balance, measured its Vickers hardness using a Vickers hardness tester (HV30, with a pressure time of 15 seconds), measured its bending strength using a tensile testing machine, and measured its coercivity using a coercivity meter.

 

Experimental data on TaC carbide

The microstructure of the TaC carbide?material obtained is shown in Figure 1.

sample pic of TaC carbide

From Figure 2, it can be seen that at a sintering temperature of 1425°C, the grain size mainly distributed in ultra-fine grains, showing a normal distribution. At a sintering temperature of 1450°C, the grain size was concentrated in adjacent ultra-fine and ultra-submicron grains, accounting for nearly 70% of the total statistics. The number of nanocrystals also reached its highest value.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 2

At a sintering temperature of 1500°C, the grain size mainly distributed in ultra-fine grains, but some grains grew significantly, resulting in a decrease in the proportion of nanocrystals and ultra-submicron grains, and an increase in the proportion of medium-sized and coarse grains, resulting in a more scattered grain size distribution.

 

Experimental result analysis

The impact of sintering temperature on mechanical properties

The microstructure and properties of the TaC carbide material obtained are shown in Figure 2, where the bending strength and hardness of the sample increase with the increase of sintering temperature. Therefore, when sintered at 1500°C, the TaC carbide grain size continues to grow. From Figure 3, it can be seen that with the increase of sintering temperature, the bending strength value slightly increases.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 3

The bending strength of the carbide?increases as the uniformity of the WC average grain size improves. When the sample is sintered at 1450°C, the average grain size distribution is uniform, and the bending strength slightly increases. When sintered at 1500°C, the excessively high sintering temperature causes the WC grains to grow through the dissolution-precipitation process, and the increase in grain size is beneficial to improve the bending strength of the carbide. However, overall, the change in bending strength value from 914 MPa to 1081 MPa with the increase in temperature is not very significant.

 

 

The effect of sintering temperature on density and coercivity

Figure 4 shows the variation curves of density and coercivity of the samples with the change of sintering temperature. Density is one of the important physical properties of powder metallurgical materials, and the change of compact size during sintering is closely related to the change of density.

The 3 Aspects that Sintering Temperature Influence Tac Carbide 4

At 425 ℃ sintering, the shrinkage is incomplete and there are voids present, resulting in a lower density value. With the increase of sintering temperature, the flowability of the bonding phase improves, which is beneficial to eliminate pores and increase the density of the carbide.

When the temperature rises to 1,500 ℃, the volatilization of Co leads to a decrease in the amount of liquid phase, which is not conducive to pore filling, resulting in a decrease in density value.

 

As for coercivity, in WC-Co carbides, the coercivity is mainly related to the Co content and its dispersion. When non-magnetic η-phase appears in the carbide, the coercivity will increase due to the corresponding reduction in the amount of Co phase and the refinement of WC grains. In carbides with normal microstructure, as the carbon content decreases, the tungsten content in the Co phase increases, which strengthens the Co phase and increases the coercivity. At 1450 ℃ sintering, the grains of the sample are refined and evenly distributed, which maximizes the dispersion of the Co phase and thus maximizes the coercivity.

Conclusion

In this study, TaC?carbides were prepared using WC raw materials with different particle sizes and sintered at different temperatures. The following conclusions were drawn:

  1. Under the experimental conditions, the hardness, density, and coercivity of the carbideall first increase and then decrease with the temperature, and the sintering temperature has little effect on the bending strength of the carbide. When sintered at 1450 ℃ and held for 1.5 h, the comprehensive performance of the carbide?is the best, with a Vickers hardness (HV30) of 1668.8, a bending strength of 988 MPa, a density of 14.87 g/cm3, and a coercivity of 15.2 kA/m.
  2. When using mixed particle size WC, TaC has the best inhibitory effect on WC grain at 1450 ℃.

Leave a Reply

Your email address will not be published. Required fields are marked *

国产欧美洲中文字幕床上| 操的我的逼逼好爽好多水| 骚逼嫩鸡巴喷水视频| 无码爆一二三区免费视频| 成人国产亚洲精品一区二| 午夜精品在线视频| 西瓜在线看免费观看视频| 国产成人精品免费视频全| 欧美一区二区三区四区五区精品| 欧美精品一区二区三区四区五区| 欧美一区二区三区高清性群p| 亚洲午夜av一区二区三区| 性一交一子一伦一乱| 夜夜38亚洲综合网| 巨屌抽插舔阴视频| 亚欧日韩国产在线| 日本中文字幕无人区一区二区| 欧美人人做人人爽人人喊| 欧美激情在线播放第一页| 欧美一级淫片免费播放口| 日本欧美中文字幕| 亚洲综合区欧美一区二区| 两人爽爽爽无码免费视频| 国产一级第一级毛片| 几巴怪物操逼视频| 国产一区曰韩二区欧美三区| 日韩在线中文字幕在线视频| AV无码超清破解版流出| 中文字幕乱码一区三区免费| 欧美亚洲熟妇视频在线观看| 有关日本黄色录像的视频| 黑人猛操日本美女| 大逼女人污污视频| 操美女干逼调教捆绑视频| 亚洲高清中文字幕一区二区三区| 欠欠草免费在线视频| 国产天美传媒剧免费观看| 国产高欧美性情一线在线| 黑人大鸡巴日小逼| 免费黄色 操逼视频| 喜欢被粗大阴茎插入|